Method for producing r-t-b sintered magnet
During the manufacturing process of R-T-B system sintered magnets, the alloy powder and molded body are immersed in the oil agent to control the dissolved oxygen amount, and the problem of reduced density and coercivity caused by the oxidation of rare earth elements is solved, and high density and low deformation are achieved sintered body.
Patent Information
- Application Number
- CN202380029841.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-24
- Filing Date
- 2023-02-22
- Publication Date
- 2024-11-15
AI Technical Summary
When increasing the ratio of R2T14B square crystal compound in the main phase of R-T-B sintered magnet, it is easy to cause oxidation of rare earth elements, resulting in the problem of reducing density, reducing coercive force (HcJ) and deformation.
By immersing the R-T-B alloy powder and the molded body in the oil agent solution for storage, the dissolved oxygen amount in the oil agent is controlled to be less than 2.5 mg/l, and the oxidation reaction is inhibited, thereby reducing the increase in oxygen concentration and preventing density reduction and deformation.
It effectively reduces the oxidation of R-T-B-type sintered magnets, improves density and coercivity, reduces deformation, and ensures a high-performance sintered body.
Smart Images

Figure CN118974858A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing an RTB based sintered magnet. Background Art
[0002] RTB sintered magnets (R is a rare earth element, which must contain at least one selected from Nd, Pr and Ce, T is at least one selected from Fe, Co, Al, Mn and Si, which must contain Fe, and B is boron) include R2Fe 14 The main phase of the compound with B-type crystal structure, the grain boundary phase located at the grain boundary of the main phase, and the compound phase generated by the influence of trace added elements and impurities. RTB system sintered magnets show high residual flux density B r (hereinafter sometimes referred to as "B r ”) and high coercivity H cJ (hereinafter sometimes referred to as "H cJ ”), is known to be the highest performance permanent magnet.
[0003] Therefore, RTB-based sintered magnets are used in engines in various fields such as electric vehicles (EV, HV, PHV), renewable energy fields such as wind power generation, home appliances, and industrial fields. RTB-based sintered magnets are indispensable materials for the miniaturization / lightweighting, high efficiency / energy saving (improvement of energy efficiency) of these engines. In addition, by using RTB-based sintered magnets in drive motors for electric vehicles, the replacement of internal combustion engine vehicles with electric vehicles is achieved, which also helps to prevent global warming by reducing greenhouse gases such as carbon dioxide (reduction of fuel / exhaust). In this way, RTB-based sintered magnets have made a significant contribution to the realization of a clean energy society. In addition, RTB-based sintered magnets are usually prepared by crushing, molding, sintering, etc. of RTB-based sintered alloys.
[0004] RTB sintered magnets can be obtained by increasing the R2T 14 The existence ratio of tetragonal compounds of B is used to increase the r In addition, although the grain boundary phase (such as R-rich phase) needs to have a minimum content for liquid phase sintering, since R reacts with oxygen in the atmosphere to generate oxides such as R2O3, some R is consumed in the part that does not contribute to sintering. Therefore, when a large amount of oxides are generated, the amount of R required for sintering is insufficient, which sometimes reduces the density of the RTB-based sintered magnet obtained after sintering. In addition, H cJ Furthermore, insufficient R may cause poor shrinkage, thereby causing deformation of the RTB based sintered magnet.
[0005] The higher the oxygen concentration in the RTB-based sintered alloy powder before sintering and the molded body obtained by compression molding the RTB-based alloy powder, the more significant the generation of oxides becomes. Therefore, it is necessary to reduce the oxygen concentration in the RTB-based alloy powder and the molded body.
[0006] Patent Document 1 describes mixing raw material powder for rare earth sintered magnet (equivalent to RTB alloy powder) with mineral oil and the like and wet molding the mixture. By mixing the raw material powder for rare earth sintered magnet with mineral oil and the like, direct contact between the raw material powder for rare earth sintered magnet and oxygen in the atmosphere can be suppressed, thereby reducing the oxygen concentration in the raw material powder for rare earth sintered magnet.
[0007] Patent Documents 2 and 3 propose a method of placing the obtained molded body into an organic solvent in a tank after molding an alloy powder (equivalent to RTB alloy powder). By placing the obtained molded body into an organic solvent, the molded body is covered with the organic solvent, so that direct contact between the molded body and oxygen in the atmosphere can be suppressed, and the oxygen concentration in the molded body can be reduced.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Laid-Open No. 7-57914
[0011] Patent Document 2: Japanese Patent Application Publication No. 2002-8935
[0012] Patent Document 2: Japanese Patent Application Publication No. 2002-170728 Summary of the invention
[0013] Technical problem to be solved by the invention
[0014] In recent years, in order to achieve higher performance, research has been conducted to make the main phase R2T 14 The existence ratio of tetragonal compounds of B increases. When the existence ratio of the main phase is increased, it is more likely to cause R deficiency due to oxidation. Therefore, it is necessary to further reduce the oxygen concentration in the RTB alloy powder and the molded body. To this end, an embodiment of the present invention provides a method for further reducing the oxygen concentration in the RTB alloy powder and the molded body, suppressing the decrease in the density of the RTB sintered magnet, and preventing the RTB sintered magnet from being oxidized. cJ A method for producing a sintered RTB magnet that reduces the deformation of the RTB magnet.
[0015] Technical solutions for solving technical problems
[0016] The manufacturing method of the RTB-based sintered magnet of the present invention includes, in the illustrated embodiment: a pulverizing step of pulverizing an RTB-based alloy to prepare an RTB-based alloy powder (R is a rare earth element and must contain at least one selected from Nd, Pr and Ce, T is Fe or Fe and Co, and B is boron); a powder storage step of immersing the above-mentioned RTB-based alloy powder into a solution tank containing an oil agent to store the above-mentioned RTB-based alloy powder; a molding step of compression molding the RTB-based alloy powder after the above-mentioned powder storage step to prepare a molded body; and a sintering step of sintering the above-mentioned molded body, when the dissolved oxygen content of the oil agent in the above-mentioned solution tank in the above-mentioned powder storage step is set to Do, it satisfies Do<2.5mg / l.
[0017] In certain embodiments, Do<1.0 mg / l is satisfied.
[0018] In certain embodiments, the method comprises: a molding process of compressing RTB alloy powder (R is a rare earth element and must contain at least one selected from Nd, Pr and Ce, T is Fe or Fe and Co, and B is boron) to prepare a molded body; a molded body storage process of immersing the above-mentioned molded body in a solution tank added with an oil agent to store the above-mentioned molded body; and a sintering process of sintering the molded body after the above-mentioned molded body storage process, when the dissolved oxygen content of the oil agent in the solution tank in the above-mentioned molded body storage process is set to Do, Do<2.5mg / l is satisfied.
[0019] In certain embodiments, Do<1.0 mg / l is satisfied.
[0020] In another exemplified embodiment, the method for manufacturing an RTB-based sintered magnet of the present invention includes: a pulverizing step of pulverizing an RTB-based alloy to prepare an RTB-based alloy powder (R is a rare earth element and must include at least one selected from Nd, Pr and Ce, T is Fe or Fe and Co, and B is boron); a powder storage step of immersing the above-mentioned RTB-based alloy powder into a first solution tank added with a first oil agent to store the above-mentioned RTB-based alloy powder; a molding step of compression molding the RTB-based alloy powder after the above-mentioned powder storage step to prepare a molded body; a molded body storage step of immersing the above-mentioned molded body into a second solution tank added with a second oil agent to store the above-mentioned molded body; and a sintering step of sintering the molded body after the above-mentioned molded body storage step, wherein the dissolved oxygen content of the first oil agent in the above-mentioned first solution tank in the above-mentioned powder storage step and the dissolved oxygen content of the first oil agent in the above-mentioned second solution tank in the above-mentioned molded body storage step are both less than 2.5 mg / l.
[0021] Effects of the Invention
[0022] According to the embodiment of the present invention, it is possible to further reduce the oxygen concentration in the RTB alloy powder and the molded body, suppress the decrease in the density of the RTB based sintered magnet, and provide cJ A method for producing a sintered RTB magnet that reduces the deformation of the RTB magnet. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a flow chart showing an example of the process of the method for producing an RTB based sintered magnet according to the present invention.
[0024] Figure 2 This is an explanatory diagram for explaining the method of measuring the deformation amount. DETAILED DESCRIPTION
[0025] The inventors have conducted a detailed study on the causes of oxidation of RTB alloy powders and molded bodies. As a result, it can be seen that after preparing RTB alloy powders and molded bodies, oxidation (increase in oxygen concentration) will occur while waiting for the process of preparing these products to proceed to the next process. Among them, the next process of the process of preparing RTB alloy powders is a molding process. In addition, the next process of the process of preparing molded bodies is a sintering process. The inventors believe that in order to prevent such oxidation, it is necessary to immerse the RTB alloy powders and molded bodies in a solution tank filled with oil immediately after preparing them for storage. And it is known that according to this method, the oxygen concentration of RTB alloy powders and molded bodies is not increased compared to the case where they are not immersed in the oil, but the oxygen concentration of RTB alloy powders and molded bodies immersed in the oil increases during storage. This means that even if immersed in oil, the oxidation of RTB alloy particles still proceeds. After further research based on these insights, the inventors found that by setting the amount of dissolved oxygen in the oil in the solution tank to below a specific amount, the increase in the oxygen concentration of RTB alloy powders and molded bodies can be greatly suppressed. Generally, no matter what kind of oil, a small amount of oxygen will be dissolved. Even if the content of dissolved oxygen is extremely small, the oxidation of RTB alloy powder and molded body due to dissolved oxygen will still proceed, but the increase in oxygen concentration is only about tens of ppm. However, it can be seen that: when the oxygen dissolved in the oil is consumed, new oxygen will be introduced from the contact surface between the oil and the atmosphere, so that oxidation continues, resulting in an increase in the oxygen concentration of RTB alloy powder and molded body.
[0026] If the RTB alloy powder and the molded body are not stored in an oil, but are stored in a nitrogen atmosphere to block their contact with oxygen, the oxidation can be suppressed. However, in order to make the entire device in a nitrogen atmosphere, it is necessary to cover the entire device and carry out nitrogen flow, and the equipment becomes large and complicated. In addition, airtightness is also required, so there will be problems such as the equipment itself is difficult to operate and poor maintainability. In addition, if the RTB alloy powder and the molded body are molded and sintered in a short time without storage, the oxidation can be suppressed because the contact time with oxygen is short. However, since a certain amount of molded bodies are sintered at one time in the usual sintering process, there will be a waiting time required until a certain amount of molded bodies are completed.
[0027] Therefore, the inventors of the present invention considered to suppress the progress of oxidation by reducing the oxygen dissolved in the oil. Specifically, by setting the dissolved oxygen content Do of the oil in which the RTB alloy powder or the molded body is impregnated to 2.5 mg / l or less, the progress of oxidation of the RTB alloy powder and the molded body can be suppressed, and the density reduction of the sintered body after sintering, the H cJ The oxygen dissolved in the oil depends on the liquid temperature of the oil and the oxygen partial pressure of the atmosphere in contact. It was found that, for example, by inserting a hose into the solvent and introducing nitrogen gas through the hose to reduce the oxygen partial pressure around the oil (solvent), the dissolved oxygen can be reduced. According to this method, it is easier to block oxygen than to place the entire device under a nitrogen atmosphere.
[0028] (RTB sintered magnet)
[0029] The RTB based sintered magnet of the present invention has, for example, the following composition.
[0030] contain:
[0031] R: 27-35% by mass
[0032] B: 0.80-1.20% by mass
[0033] Ga: 0-1.0 mass %
[0034] Cu: 0-0.5% by mass
[0035] T: 60 mass % or more.
[0036] (R: 27-35 mass %)
[0037] R is a rare earth element and must contain at least one selected from Nd, Pr and Ce. When R is less than 27% by mass, liquid phase may not be fully generated during sintering, making it difficult to fully achieve densification of the sintered body. On the other hand, when R exceeds 35% by mass, grain growth may occur during sintering, and H cJ The content of R is preferably 29.5 to 33.0% by mass. When R is within this range, a higher B r As R, a heavy rare earth element RH such as Tb, Dy, or Ho may be contained.
[0038] (B: 0.80 to 1.20 mass %)
[0039] When B is less than 0.80 mass %, there is a possibility that B r On the other hand, when B exceeds 1.20 mass%, H cJ The content of B is preferably 0.88 to 0.90 mass %. When B is within this range, a higher H cJ .
[0040] (Ga: 0-1.0 mass%)
[0041] The Ga content is preferably 0 to 1.0 mass %, more preferably 0.2 to 0.7 mass %. When Ga is within this range, a higher H cJ .
[0042] (Cu: 0 to 0.50 mass%)
[0043] The content of Cu is preferably 0 to 0.50 mass %, more preferably 0.05 to 0.30 mass %. When Cu is within this range, a higher H cJ .
[0044] (T: 60 mass % or more)
[0045] T is Fe or Fe and Co.
[0046] The T content in the sintered magnet is preferably 61.5 to 69.5% by mass. In addition, when the total amount of T is set to 100% by mass, less than 10% by mass can be replaced by Co. For example, 90% by mass of the total amount of T can be Fe and 10% by mass can be Co. In addition, the total amount of T (100% by mass) can also be Fe. The inclusion of Co can improve the corrosion resistance, but when the substitution amount of Co exceeds 10% by mass of Fe, it may not be possible to obtain a high B r .
[0047] The RTB based sintered magnet of the present invention may further contain any other elements.
[0048] An embodiment of the method for producing an RTB based sintered magnet according to the present invention will be described below. Figure 1 FIG. 1 is a flow chart showing an example of the process of producing a sintered RTB magnet according to the present invention. Figure 1 As shown in the flowchart, the RTB system sintered magnet manufacturing method of the present invention includes:
[0049] A pulverizing step (S10) for preparing RTB alloy powder;
[0050] A molding step (S20) of compressing the RTB alloy powder to prepare a molded body; and
[0051] a sintering step (S30) of sintering the molded body,
[0052] A powder storage step (S100) and / or a
[0053] A molded body storage step ( S200 ) is included between the molding step ( S20 ) and the sintering step ( S30 ).
[0054] The powder storage step (S100) and the molded body storage step (S200) may be both performed, or only at least one of the steps may be performed. That is, the embodiment of the method for producing an RTB-based sintered magnet of the present invention may be a method for producing an RTB-based sintered magnet comprising a pulverizing step (S10), a powder storage step (S100), a molding step (S20), and a sintering step (S30), or a method for producing an RTB-based sintered magnet comprising a pulverizing step (S10), a molding step (S20), a molded body storage step (S200), and a sintering step (S30), or a method for producing an RTB-based sintered magnet comprising a pulverizing step (S10), a powder storage step (S100), a molding step (S20), a molded body storage step (S200), and a sintering step (S30).
[0055] Hereinafter, each of these steps will be described in more detail.
[0056] (1) Pulverization process for preparing RTB alloy powder
[0057] According to the target composition, metals or alloys of each element are prepared, and these are subjected to a thin strip casting method or the like to produce an RTB alloy. The obtained RTB alloy is subjected to hydrogen pulverization to reduce the size of the coarse pulverized powder to, for example, 1.0 mm or less. Next, the coarse pulverized powder is finely pulverized using a jet mill or the like to obtain, for example, a median particle size d 50The finely pulverized powder (RTB alloy powder) is 2.0 μm ≤ d50 ≤ 8.0 μm (value obtained by laser diffraction method using air flow dispersion method). The particle size d of the RTB alloy powder is preferably 50 2.0 μm ≤ d50 ≤ 5.0 μm. By setting it within this range, the magnetic properties can be further improved. When the particle size is reduced, the RTB alloy powder becomes easily oxidized. Therefore, in order to suppress the particle size d 50 The oxidation of RTB alloy powders in the range of 2.0μm≤d50≤5.0μm and molded bodies containing the same is extremely effective using the method of the present invention. It should be noted that a known lubricant can be used as an auxiliary agent in the coarsely crushed powder before jet mill pulverization, in the jet mill pulverization, and in the RTB alloy powder after jet mill pulverization. d50 can be measured by airflow dispersion laser diffraction method (according to JIS Z 8825: 2013 revised edition). That is, in the present invention, d 50 It refers to the particle size (median diameter) when the cumulative particle size distribution (volume basis) from the smaller particle size side reaches 50%.
[0058] (Powder storage process)
[0059] The obtained RTB alloy powder is immersed in a solution tank containing an oil agent to store the RTB alloy powder. The solution tank refers to a tank containing an oil agent, and there is no special requirement for the shape and size of the solution tank. As long as the shape and size can be used to immerse the RTB alloy powder, the oil agent can use mineral oil, petroleum solvents represented by isoparaffin, cycloparaffin solvents, etc.
[0060] The present invention is characterized in that, in a solution tank immersed with RTB alloy powder, when the amount of dissolved oxygen in the oil in the solution tank is set to Do, Do<2.5 mg / l is satisfied. The oxidation of the RTB alloy powder can be suppressed, and the density reduction of the sintered body after sintering can be suppressed. cJ The amount of dissolved oxygen in the oil in the solution tank preferably satisfies Do<1.0 mg / l. The oxidation of the RTB alloy powder can be more reliably suppressed.
[0061] As described above, reducing the dissolved oxygen in the solvent in the solution tank can be achieved in the following ways, for example, by inserting a hose into the solvent and introducing nitrogen through the hose to reduce the oxygen partial pressure around the oil. It should be noted that the hose can be made of rubber, plastic, metal, etc., and the material is not limited. In addition to nitrogen, well-known inactive gases such as argon can also be used. The amount of dissolved oxygen in the oil can be determined by well-known methods. For example, a dissolved oxygen analyzer using a nuclear membrane type galvanic cell oxygen sensor can be used. The oxygen sensor can also be used to monitor the dissolved oxygen in the solvent, for example, regularly, and when the dissolved oxygen content reaches a baseline value (for example, 1.0 mg / l), nitrogen is introduced into the solvent.
[0062] (2) Molding process
[0063] The RTB alloy powder after the powder storage process is subjected to compression molding to prepare a molded body. The RTB alloy powder is molded in a magnetic field to obtain a molded body. The molding in the magnetic field can be performed by any known molding method in the magnetic field, including a dry molding method in which dry alloy powder is injected into the mold cavity of the mold and molding is performed while applying a magnetic field, and a wet molding method in which a slurry dispersed with the alloy powder is injected into the mold cavity of the mold and molding is performed while discharging the dispersion medium of the slurry.
[0064] (3) Molded body storage process
[0065] The molded body is stored by immersing it in a solution tank containing an oil agent. There are no special requirements for the shape and size of the solution tank. As long as the shape and size can be immersed in the molded body, it will suffice. The oil agent can use the same type of solvent as the oil agent used in the above-mentioned powder storage step. The present invention is characterized in that in the solution tank in which the molded body is immersed, when the dissolved oxygen content of the oil agent in the solution tank is set to Do, Do<2.5mg / l is satisfied. The oxidation of the molded body can be suppressed, and the density reduction of the sintered body after sintering and the H cJ reduction and deformation. The dissolved oxygen content of the oil in the solution tank preferably satisfies Do<1.0mg / l. The oxidation of the molded body can be more reliably suppressed. The method for reducing the dissolved oxygen of the solvent in the solution tank can adopt the same method as the above-mentioned powder storage process. It should be noted that in the powder storage process and the molded body storage process, separate solution tanks can be used, or the same solution tank can be used. When using separate solution tanks, different solvents can be used. The solution tank used in the powder storage process can be called the first solution tank, and the solution tank used in the molded body storage process can be called the second solution tank, but the first solution tank and the second solution tank can also be the same structure.
[0066] (4) Sintering process
[0067] The molded body after the molded body storage process is sintered. The sintering of the molded body is preferably carried out at a temperature range of 950°C to 1150°C. In order to prevent oxidation caused by sintering, the residual gas in the atmosphere can be replaced with an inactive gas such as helium or argon. The obtained sintered body is preferably heat-treated. The magnetic properties can be improved by heat treatment. The heat treatment conditions such as heat treatment temperature and heat treatment time can adopt known conditions. As needed, the RTB system sintered magnet obtained in this way can be subjected to a grinding / polishing process, a surface treatment process and a magnetization process, etc., to finally obtain an RTB system sintered magnet.
[0068] In certain preferred embodiments, the method for producing an RTB-based sintered magnet of the present invention further includes a diffusion step of diffusing an alloy containing a heavy rare earth element RH (RH is at least one of Tb, Dy, and Ho) or an alloy containing R and M (M is at least one selected from Ga, Cu, Zn, Al, and Si) (RM alloy) from the surface of the sintered body to the interior. When the heavy rare earth elements RH, R, and M (Ga, Cu, etc.) are diffused from the surface of the sintered body to the interior, the coercive force can be effectively improved.
[0069] Example
[0070] The RTB based sintered magnet of the present invention will be described in more detail using experimental examples, but the present invention is not limited to these examples.
[0071] Experimental Example 1
[0072] Each element was weighed so that the RTB-based sintered body had the composition shown in Table 1, and was cast by a thin strip continuous casting method to obtain a flaky alloy. The obtained alloy was subjected to hydrogen pulverization, and then subjected to a dehydrogenation treatment by heating and cooling to 550°C in a vacuum to obtain a coarsely pulverized powder. Next, 0.05% by mass of zinc stearate as a lubricant was added to the obtained coarsely pulverized powder relative to 100% by mass of the coarsely pulverized powder, and after mixing, an airflow pulverizer (jet pulverizer device) was used to dry-pulverize in a nitrogen flow to obtain a finely pulverized powder (RTB-based alloy powder) with a particle size D50 of 4.5 μm. It should be noted that the particle size D50 is the volume center value (volume-based median particle size) obtained by a laser diffraction method using an airflow dispersion method.
[0073] A hydrocarbon lubricant as a lubricant is added to the above RTB alloy powder in an amount of 1.6% by mass relative to 100% by mass of the finely pulverized powder, mixed, and then immersed in a solution tank containing an oil agent. The dissolved oxygen content of the oil agent during immersion is 9.1 mg / l. A hose is inserted into the solvent and nitrogen gas is introduced from the hose. The dissolved oxygen content is controlled to 0.8 to 9.1 mg / l by adjusting the flow rate of the introduced nitrogen gas. It should be noted that the dissolved oxygen content in the oil agent is measured using a dissolved oxygen analyzer using a diaphragm-type galvanic oxygen sensor (organic solvent-compatible dissolved oxygen meter B-506S manufactured by Iijima Electronics Co., Ltd.). Then, after immersing the RTB alloy powder in the solution tank, the finely pulverized powder of the RTB alloy powder is stored in the oil agent for 0 to 24 hours while the dissolved oxygen content is kept constant. The RTB alloy powder after storage is molded in a magnetic field to obtain a molded body. It should be noted that the molding device used was a so-called right-angle magnetic field molding device (transverse magnetic field molding device) in which the magnetic field application direction was orthogonal to the pressurization direction.
[0074] The obtained molded body was sintered at 1050°C for 4 hours in an Ar gas flow and then rapidly cooled to obtain an RTB system sintered magnet. The composition of the RTB system sintered magnet (before the diffusion process) is shown in Table 1. The dimensions of the RTB system sintered magnet during molding were about 18 mm in the direction of the applied magnetic field, about 10 mm in the direction of the pressure, and about 48 mm in other directions. The obtained RTB system sintered magnet was machined to produce a sample with a length of 7.2 mm, a width of 7.2 mm, and a thickness of 7.2 mm. The obtained sample was coated with 2.0 mass% of a Pr-Ga alloy powder prepared by an atomization method with a composition shown in Table 2 relative to 100 mass% of the RTB system sintered magnet, and then kept at 900°C for 10 hours in an Ar gas flow, and then subjected to heat treatment to cool to room temperature, and a diffusion process was performed. Subsequently, the sample was kept at 470°C for 3 hours in an Ar gas flow, and then subjected to heat treatment to cool to room temperature, to obtain an RTB system sintered magnet (No. 1 to 9). The oxygen content and deformation amount of the obtained RTB based sintered magnet are shown in Table 3. The oxygen content was measured using a gas analyzer using a gas fusion-infrared absorption method. Figure 2 This is an illustration of the method for measuring the deformation amount. Figure 2 The dimensions of the center A and the end B of the RTB system sintered magnet before machining shown in the figure were measured in the direction of magnetic field application M during molding, and the difference was taken as the deformation amount. The RTB system sintered magnets (No. 1 to 9) after heat treatment were respectively machined to prepare samples with a length of 7.0 mm, a width of 7.0 mm, and a thickness of 7.0 mm, and the magnetic properties of each sample were measured by a BH tracer. The measurement results are shown in Table 3.
[0075] [Table 1]
[0076]
[0077] [Table 2]
[0078]
[0079] [Table 3]
[0080]
[0081] As shown in Table 3, all the examples within the scope of the present invention have an oxygen content as low as 0.144 mass % or less and a sintered body density of 7.57 g / cm 3 Above, and deformation less than 0.50mm, H cJ :High density above 1824KA / m, high H cJ In contrast, No. 1 to 6, whose dissolved oxygen was outside the range of the present invention, failed to obtain high density and H cJ In addition, as the storage time increases, the oxygen content increases, the density and H cJ Decreases and deformation increases.
[0082] Experimental Example 2
[0083] Each element was weighed so that the RTB-based sintered body had the composition shown in Table 4, and was cast by a thin strip continuous casting method to obtain a flaky alloy. The obtained alloy was hydrogen-crushed, and then subjected to a dehydrogenation treatment by heating and cooling to 550°C in a vacuum to obtain a coarsely pulverized powder. Next, 0.08% by mass of a hydrocarbon-based lubricant was added to the obtained coarsely pulverized powder relative to 100% by mass of the coarsely pulverized powder, and after mixing, an airflow pulverizer (jet pulverizer device) was used to dry-crush it in a nitrogen flow to obtain a finely pulverized powder (RTB-based alloy powder) with a particle size D50 of 3.0 μm. It should be noted that the particle size D50 is the volume center value (volume-based median particle size) obtained by a laser diffraction method using an airflow dispersion method.
[0084] A hydrocarbon lubricant and an oil agent as lubricants were added to the RTB alloy powder in an amount of 0.6 mass % and 33.3 mass % respectively relative to 100 mass % of the finely pulverized powder, mixed, and then compressed in a magnetic field to obtain a molded body. It should be noted that the molding device used a so-called right-angle magnetic field molding device (transverse magnetic field molding device) in which the magnetic field application direction is orthogonal to the pressurization direction.
[0085] The obtained molded bodies No. 10 to 13 are placed in the atmosphere, and the obtained molded bodies No. 14 to 22 are immersed in a solution tank containing an oil agent, and the molded bodies are stored in the oil agent. A hose is inserted into the solvent and nitrogen gas is introduced from the hose. The dissolved oxygen content is controlled at 0 to 8.4 mg / l by adjusting the flow rate of the introduced nitrogen gas. The stored molded bodies are sintered in an Ar gas flow at a temperature of 1040°C for 4 hours and then rapidly cooled to obtain RTB-based sintered magnets. The composition of the RTB-based sintered magnet (before the diffusion process) is shown in Table 4. The sintered bodies No. 14 to 22 were respectively machined to prepare samples with a length of 7.2 mm, a width of 7.2 mm, and a thickness of 7.2 mm. The obtained samples were coated with 3.0 mass% of the Pr-Ga alloy powder prepared by the atomization method with the composition shown in Table 5 relative to 100 mass% of the RTB system sintered magnet, and then kept at 900°C for 10 hours in an Ar gas flow, and then subjected to heat treatment after cooling to room temperature, and a diffusion process was performed. Subsequently, the samples were kept at 500°C for 1 hour in an Ar gas flow, and then subjected to heat treatment after cooling to room temperature, thereby obtaining RTB system sintered magnets (No. 14 to 22). The oxygen content and deformation of the obtained RTB system sintered magnets are shown in Table 6. It should be noted that the oxygen content was measured using a gas analyzer using a gas melting-infrared absorption method. The deformation was measured by measuring the dimensions of the center and end of the sintered magnet, and the difference was taken as the deformation. The RTB system sintered magnets (No. 14 to 22) after heat treatment were respectively machined to prepare samples with a length of 7.0 mm, a width of 7.0 mm, and a thickness of 7.0 mm, and the magnetic properties of each sample were measured by a BH tracer. The measurement results are shown in Table 6.
[0086] [Table 4]
[0087]
[0088] [Table 5]
[0089]
[0090] [Table 6]
[0091]
[0092] As shown in Table 6, all the examples within the scope of the present invention have an oxygen content as low as 0.088 mass % or less and a sintered body density of 7.58 g / cm 3 Above, and deformation less than 0.50mm, H cJ : High density and high H above 2060KA / m cJ In contrast, No. 14 to 19, whose dissolved oxygen was outside the range of the present invention, failed to obtain high H cJIn addition, as the storage time increases, the oxygen content increases, the density and H cJ It should be noted that the deformation amounts of No. 10 to 13 were large, making it difficult to perform machining.
Claims
1. A method for producing a RTB based sintered magnet, characterized in that: include: A pulverizing step of pulverizing an RTB alloy to prepare an RTB alloy powder, wherein R is a rare earth element and must include at least one selected from Nd, Pr and Ce, T is Fe or Fe and Co, and B is boron; A powder storage step of immersing the RTB alloy powder in a solution tank containing an oil agent to store the RTB alloy powder; A molding step of compression molding the RTB alloy powder after the powder storage step to prepare a molded body; and a sintering step of sintering the molded body, When the amount of dissolved oxygen in the oil solution in the solution tank in the powder storage step is defined as Do, Do<2.5 mg / l is satisfied.
2. The method for producing a RTB based sintered magnet according to claim 1, wherein: Satisfy Do<1.0mg / l.
3. A method for producing a RTB based sintered magnet, characterized in that: include: A molding process of preparing a molded body by compression molding RTB alloy powder, wherein R is a rare earth element and must contain at least one selected from Nd, Pr and Ce, T is Fe or Fe and Co, and B is boron; A molded body storage step of immersing the molded body in a solution tank containing an oil agent to store the molded body; and a sintering step of sintering the molded body after the molded body storage step, When the amount of dissolved oxygen in the oil solution in the solution tank in the molded body storage step is defined as Do, Do<2.5 mg / l is satisfied.
4. The method for producing a RTB based sintered magnet according to claim 3, wherein: Satisfy Do<1.0mg / l.
5. A method for producing a RTB based sintered magnet, characterized in that: include: A pulverizing step of pulverizing an RTB alloy to prepare an RTB alloy powder, wherein R is a rare earth element and must include at least one selected from Nd, Pr and Ce, T is Fe or Fe and Co, and B is boron; A powder storage step of immersing the RTB alloy powder in a first solution tank containing a first oil agent to store the RTB alloy powder; A molding step of compressing and molding the RTB alloy powder after the powder storage step to prepare a molded body; A molded body storage step of immersing the molded body in a second solution tank containing a second oil agent to store the molded body; and a sintering step of sintering the molded body after the molded body storage step, The amount of dissolved oxygen in the first oil agent in the first solution tank in the powder storage step and the amount of dissolved oxygen in the first oil agent in the second solution tank in the molded body storage step are both lower than 2.5 mg / l.