Recyclable MFe2O4-coated GA catalyst as well as preparation method and application thereof

By preparing cyclable catalysts in solid-loaded MFe2O4 nanoparticles in graphene hydrogels and applying them in micro-nanogas-liquid dispersion systems, the problems of low catalyst recycling rate and insufficient denitrification efficiency are solved, and efficient NOx and SO2 are achieved Removal and environmentally friendly use of catalysts.

CN118976495APending Publication Date: 2024-11-19DONGHUA UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411057676.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The recycling rate of existing catalysts in flue gas treatment is not high, and the traditional wet denitrification technology has the problems of slow gas-liquid mass transfer rate and low denitrification efficiency, which affects the effective treatment of NOx.

Method used

The MFe2O4 nanoparticles are solidly loaded on graphene hydrogel and prepared by vacuum freeze-drying, and are used in micro-nanogas-liquid dispersion systems to perform catalytic oxidation of NOx and SO2 using high-energy reaction field and reactive oxygen. .

Benefits of technology

It realizes efficient NOx and SO2 removal, the catalyst can be recycled, no metal ion leaching, and the absorbent liquid can be recycled, avoiding secondary pollution, and improving the efficiency and environmental protection performance of flue gas treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976495A_ABST
    Figure CN118976495A_ABST
Patent Text Reader

Abstract

The invention relates to a recyclable MFe2O4-coated GA catalyst as well as a preparation method and application thereof. The recyclable MFe2O4-coated GA catalyst is prepared by immobilizing MFe2O4 nanoparticles in graphene hydrogel and carrying out vacuum freeze drying, wherein M is one of Mn, Co, Ni, Cu and Zn. The recyclable MFe2O4 (at) GA catalyst is coupled with a micro-nano bubble absorption flue gas system, so that the system has the advantages that the catalyst utilization rate is high, the catalyst can be recycled, and no metal ions are leached; the final absorption liquid is a nitric acid solution and a sulfuric acid solution with relatively high concentration and can be recycled, so that secondary pollution is avoided; the method can realize integrated desulfurization and denitrification, and has good application prospects and industrialization potential in the field of environmental protection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of catalysts, and in particular relates to a recyclable MFe2O4@GA catalyst and a preparation method and application thereof. Background Art

[0002] NO x As the main air pollutant, SO2 has an increasing global direct emission year by year, becoming an important factor in inducing photochemical smog, causing acid rain and destroying the ozone layer, thus causing serious harm to human health. Among them, SO2 is easily soluble in water and easier to handle, while NOx is difficult to dissolve in water and becomes the focus of the flue gas treatment process. The main components of nitrogen oxides are NO and NO2, and high-valent compounds (N2O3, N2O5, etc.) with smaller contents. Traditional wet denitrification technology has the disadvantages of slow gas-liquid mass transfer rate and low denitrification efficiency. With the development of NO x The emission requirements of NO x The governance of the country faces new challenges.

[0003] Among the studied skeleton carriers, carbon-based materials have become the first choice for carrier materials due to their large specific surface area, wide application range, controllable surface structure and the function of promoting catalyst activity. Recently, graphene materials, such as graphene oxide (GO) and reduced graphene oxide (RGO), have been used as new carriers for nanoparticle catalysts. Graphene aerogels with hierarchical porous structures can greatly enhance the mass transfer efficiency of substances and promote the diffusion of reactants throughout the aerogel structure. The use of stabilizers to modify the carbon surface during the preparation process can minimize the aggregation of nanoparticles. However, the presence of stabilizers may hinder the interaction between nanoparticles and carbon skeletons. Introducing defects and oxygen-containing functional groups on the carbon skeleton can not only increase the interaction with nanoparticles, but also effectively prevent catalyst leaching. MFe2O4 nanoparticles partially dissolve in the micro-nano gas-liquid dispersion system to produce metal ions, which not only causes secondary pollution of the water body, but also affects the recycling rate of the catalyst, which limits its practical application to a certain extent. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a recyclable MFe2O4@GA catalyst and a preparation method and application thereof, so as to overcome the defects of low recycling rate of existing catalysts and poor flue gas removal effect.

[0005] The invention provides a recyclable MFe2O4@GA catalyst, which is obtained by immobilizing MFe2O4 nanoparticles in a graphene hydrogel and subjecting the catalyst to vacuum freeze-drying; wherein M is one of Mn, Co, Ni, Cu and Zn.

[0006] The present invention also provides a method for preparing a recyclable MFe2O4@GA catalyst, comprising the following steps:

[0007] (1) Using ethylene glycol as a solvent, adding MCl2·H2O and FeCl3·6H2O to stir and dissolve, then adding polyethylene glycol as a dispersant, adding sodium acetate to make the solution alkaline, transferring the solution to a hydrothermal reactor for hydrothermal reaction, washing and drying to obtain MFe2O4 nanoparticles;

[0008] (2) preparing a graphene oxide solution, adding urea as a reducing agent, and ultrasonically dispersing it; then adding MFe2O4 nanoparticles, continuing ultrasonically dispersing it, transferring the evenly dispersed solution to a hydrothermal reactor for hydrothermal reaction, and obtaining a recyclable MFe2O4@GA catalyst after vacuum freeze drying.

[0009] Preferably, the MCl2·H2O in the step (1) is one of MnCl2·H2O, CoCl2·6H2O, NiCl2·6H2O, CuCl2·2H2O, and ZnCl2·2H2O; and the molar ratio of MCl2·H2O to FeCl3·6H2O is 1:2.

[0010] Preferably, in step (1), the molar concentration of MCl2·H2O in the solution is 0.05-0.08 mol / L; the mass concentration of polyethylene glycol in the solution is 20-30 g / L; and the mass concentration of sodium acetate in the solution is 80-100 g / L.

[0011] Preferably, the hydrothermal reaction temperature in step (1) is 180-230° C., and the hydrothermal reaction time is 8-12 h.

[0012] Preferably, the initial concentration of the graphene oxide solution in step (2) is 0.5-3 mg / mL; the urea concentration is 3-6 mg / mL.

[0013] Preferably, the amount of MFe2O4 nanoparticles added in step (2) is 0.4-2 g / L.

[0014] Preferably, the hydrothermal reaction temperature in step (2) is 180-200° C., and the hydrothermal reaction time is 10-16 h.

[0015] The present invention provides an application of a circulatory MFe2O4@GA catalyst in flue gas treatment.

[0016] Furthermore, the recyclable MFe2O4@GA catalyst was placed in the reaction tower, and the NO and SO2 gases were fully mixed in the gas buffer tank to simulate the complex flue gas composition, and this was used as a gas source to pass into the micro-nano bubble generator. At the same time, distilled water was introduced into the micro-nano bubble generator to form a micro-nano gas-liquid dispersion system in the oxidation absorber to catalyze the oxidation and absorption of NO and SO2 gases.

[0017] Furthermore, during the reaction, the MFe2O4@GA catalyst and the absorption liquid were recycled, and the contents of nitrite, nitrate and sulfate in the absorption liquid were determined by ion chromatography to calculate the NO x And SO2 removal rate. The remaining flue gas is absorbed by the tail gas absorption tower.

[0018] Furthermore, the NO intake amount is 100-3000 mg / m 3 , SO2 intake volume is 100~2000mg / m 3 .

[0019] The principle of the present invention is as follows:

[0020] The MFe2O4@GA catalyst of the present invention is a three-dimensional multilayer stacked structure, and contains M=O, C=O and C–O with catalytic oxidation activity. During the micro-nano bubble rupture process, a high-energy reaction field is generated at the gas-liquid interface, triggering the generation of ·OH through the aggregation and diffusion of ions. The electrons provided by the MFe2O4 nanoparticles enhance the ability of the micro-nano bubbles to generate ·OH. The potential difference and high-energy reaction field generated by the rupture of the micro-nano bubbles cause the electrons in the catalyst to transition, and the generated O2 ·- Effectively participate in NO x In the catalytic oxidation, part of O2 ·- It will continue to gain electrons to generate ·OH, increasing the number of hydroxyl groups on the catalyst surface. The cyclic conversion between M(II) / M(III) and Fe(III) / Fe(II) ensures the catalytic activity of MFe2O4 nanoparticles. The cyclic conversion of metal ions and active oxygen in the MFe2O4 / micro-nano gas-liquid dispersion system enhances the catalytic oxidation performance of the system.

[0021] Beneficial Effects

[0022] The present invention uses the recyclable MFe2O4@GA catalyst coupled with a micro-nano bubble flue gas absorption system, which has high catalyst utilization, can be recycled, and has no metal ion leaching; the final absorption liquid is a relatively high concentration of nitric acid and sulfuric acid solution, which can be recycled and does not produce secondary pollution; integrated desulfurization and denitrification can be achieved, and it has good application prospects and industrialization potential in the field of environmental protection. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 Macroscopic image and scanning electron microscope image of the recyclable CuFe2O4@GA catalyst prepared in Example 1.

[0024] Figure 2 X-ray diffraction patterns of GO, GA and the recyclable CuFe2O4 nanoparticles prepared in Example 1.

[0025] Figure 3 Schematic diagram of the application system structure of the recyclable MFe2O4@GA catalyst of the present invention. DETAILED DESCRIPTION

[0026] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.

[0027] Example 1

[0028] S1: Weigh 5.11g CuCl2·2H2O and 16.22g FeCl3·6H2O respectively and place them in a 500mL beaker. Add 400mL ethylene glycol as solvent, then place the beaker on a magnetic stirrer and stir vigorously for 2h until the solid particles are dissolved. At this time, FeCl3·6H2O in the solution is 0.0447 W / mL. 3+ and Cu 2+ The molar ratio is 2:1. Then 10g of polyethylene glycol was added as a dispersant, and 36g of sodium acetate was added to make the solution alkaline. After continuing to stir for 30 minutes, it was evenly dispersed in the solution. The solution was transferred to a 500mL hydrothermal reactor lined with polytetrafluoroethylene and allowed to stand in a 200℃ forced air drying oven for 10 hours. After the reactor was cooled, nanoparticles were obtained. Subsequently, ethanol and deionized water were used for multiple washing to remove excess organic matter. During the washing process, a magnet was used to collect the nanoparticles to ensure the purity of the product. After the magnetically separated CuFe2O4 was dried in a vacuum oven, a high-purity CuFe2O4 magnetic nanocatalyst was obtained;

[0029] S2: Prepare a graphene oxide solution with a concentration of 2 mg / mL and add 4 mg / mL of urea as a reducing agent. Ultrasonic dispersion for 10 minutes to stably disperse the monolayer of graphene oxide in water. Add 0.05g CuFe2O4 nanoparticles and continue ultrasonic dispersion for 30 minutes. Transfer the evenly dispersed solution to a 50mL hydrothermal reactor and let it stand in an oven at 180°C for 10 hours. Cool to room temperature to obtain a graphene hydrogel containing CuFe2O4 nanoparticles. Soak the graphene hydrogel containing CuFe2O4 nanoparticles in a 20% ethanol solution for secondary structural adjustment. Take it out after 12 hours and successfully prepare a recyclable CuFe2O4@GA catalyst by freeze drying.

[0030] S3: Figure 3 As shown, the NO concentration is prepared to be 3000 mg / m 3 , SO2 volume concentration 1000mg / m 3 The mixed gas is formed into a micro-nano gas-liquid dispersion system in the reaction tower through a micro-nano bubble generator, and the above-mentioned recyclable CuFe2O4@GA catalyst is added to catalytically oxidize and absorb the complex flue gas. The concentration of nitrite and nitrate in the absorption liquid is tested using an ICS-1100 ion chromatograph to calculate the removal rates of NO and SO2.

[0031] The air intake of the micro-nano bubble generator was controlled to be 48 mL / min, the water outlet flow was 300 mL / min, and the water outlet pressure was 0.5 MPa. The volume of the reactor was 0.75 L. The cycle experiment lasted for 30 minutes, with each cycle lasting 5 minutes. The air intake was 50 mL / min at 300 mL / min, and the air intake pressure was controlled to be 0.5 MPa.

[0032] In this example, the removal rate of NO reached 76.73%, and the removal rate of SO2 reached 92.57%.

[0033] Depend on Figure 1 It can be seen that the recyclable CuFe2O4@GA material is a black cylinder with a light-weight three-dimensional porous structure.

[0034] Depend on Figure 2 It can be seen that the XRD diffraction curve of CuFe2O4@GA is consistent with the standard card of CuFe2O4, and there are characteristic peaks of reduced graphene. GO, GA and CuFe2O4@GA prepared under the optimal conditions have high crystallinity and good crystal shape.

[0035] Example 2

[0036] S1: Weigh 5.94g of MnCl2·H2O and 16.22g of FeCl3·6H2O respectively and place them in a 500mL beaker. Add 400mL of ethylene glycol as solvent, and then place the beaker on a magnetic stirrer and stir vigorously for 2h until the solid particles are dissolved. At this time, Fe 3+ and Mn 2+ The molar ratio is 2:1. Then 10g of polyethylene glycol was added as a dispersant, and 36g of sodium acetate was added to make the solution alkaline. After continuing to stir for 30 minutes, it was evenly dispersed in the solution. The solution was transferred to a 500mL hydrothermal reactor lined with polytetrafluoroethylene and allowed to stand in a 200℃ forced air drying oven for 10 hours. After the reactor was cooled, nanoparticles were obtained. Subsequently, ethanol and deionized water were used for multiple washing to remove excess organic matter. A magnet was used to collect the nanoparticles during the washing process to ensure the purity of the product. After the magnetically separated MnFe2O4 was dried in a vacuum oven, a high-purity MnFe2O4 magnetic nanocatalyst was obtained;

[0037] S2: Prepare a graphene oxide solution with a concentration of 2 mg / mL and add 4 mg / mL of urea as a reducing agent. Ultrasonic dispersion for 10 minutes to stably disperse the monolayer of graphene oxide in water. Add 0.05g of MnFe2O4 nanoparticles and continue ultrasonic dispersion for 30 minutes. Transfer the evenly dispersed solution to a 50mL hydrothermal reactor and let it stand in an oven at 180°C for 10 hours. Cool to room temperature to obtain a graphene hydrogel containing MnFe2O4 nanoparticles. Soak the graphene hydrogel containing MnFe2O4 nanoparticles in a 20% ethanol solution for secondary structural adjustment. Take it out after 12 hours and successfully prepare a recyclable MnFe2O4@GA catalyst by freeze drying.

[0038] S3: Figure 3 As shown, the NO concentration is prepared to be 3000 mg / m 3 , SO2 volume concentration 1000mg / m 3 The mixed gas is formed into a micro-nano gas-liquid dispersion system in the reaction tower through a micro-nano bubble generator, and a recyclable MnFe2O4@GA catalyst is added to catalytically oxidize and absorb the complex flue gas. The concentration of nitrite and nitrate in the absorption liquid is tested using an ICS-1100 ion chromatograph to calculate the removal rates of NO and SO2.

[0039] The air intake of the micro-nano bubble generator was controlled to be 48 mL / min, the water outlet flow was 300 mL / min, and the water outlet pressure was 0.5 MPa. The volume of the reactor was 0.75 L. The cycle experiment lasted for 30 minutes, with each cycle lasting 5 minutes. The air intake was 50 mL / min at 300 mL / min, and the air intake pressure was controlled to be 0.5 MPa.

[0040] In this example, the removal rate of NO reached 72.16%, and the removal rate of SO2 reached 93.67%.

Claims

1. A recyclable MFe2O4@GA catalyst, characterized in that: It is obtained by immobilizing MFe2O4 nanoparticles in graphene hydrogel and then subjecting to vacuum freeze-drying; wherein M is one of Mn, Co, Ni, Cu, and Zn.

2. A method for preparing a recyclable MFe2O4@GA catalyst, comprising the following steps: (1) Using ethylene glycol as a solvent, adding MCl2·H2O and FeCl3·6H2O to stir and dissolve, then adding polyethylene glycol as a dispersant, adding sodium acetate to make the solution alkaline, transferring the solution to a hydrothermal reactor for hydrothermal reaction, washing and drying to obtain MFe2O4 nanoparticles; (2) preparing a graphene oxide solution, adding urea as a reducing agent, and ultrasonically dispersing it; then adding MFe2O4 nanoparticles, continuing ultrasonically dispersing it, transferring the evenly dispersed solution to a hydrothermal reactor for hydrothermal reaction, and obtaining a recyclable MFe2O4@GA catalyst after vacuum freeze drying.

3. The preparation method according to claim 2, characterized in that: The MCl2·H2O in the step (1) is one of MnCl2·H2O, CoCl2·6H2O, NiCl2·6H2O, CuCl2·2H2O, and ZnCl2·2H2O; and the molar ratio of MCl2·H2O to FeCl3·6H2O is 1:

2.

4. The preparation method according to claim 2, characterized in that: In the step (1), the molar concentration of MCl2·H2O in the solution is 0.05-0.08 mol / L; the mass concentration of polyethylene glycol in the solution is 20-30 g / L; and the mass concentration of sodium acetate in the solution is 80-100 g / L.

5. The preparation method according to claim 2, characterized in that: The hydrothermal reaction temperature in step (1) is 180-230° C., and the hydrothermal reaction time is 8-12 h.

6. The preparation method according to claim 2, characterized in that: The initial concentration of the graphene oxide solution in step (2) is 0.5-3 mg / mL; the urea concentration is 3-6 mg / mL.

7. The preparation method according to claim 2, characterized in that: The amount of MFe2O4 nanoparticles added in step (2) is 0.4-2 g / L.

8. The preparation method according to claim 2, characterized in that: The hydrothermal reaction temperature in step (2) is 180-200° C., and the hydrothermal reaction time is 10-16 h.

9. Use of the recyclable MFe2O4@GA catalyst as claimed in claim 1 in flue gas treatment.

10. The use according to claim 9, characterized in that: The recyclable MFe2O4@GA catalyst is placed in the reaction tower, and the NO and SO2 gases are fully mixed in the gas buffer tank to simulate the complex flue gas composition, and are used as the gas source to pass into the micro-nano bubble generator. At the same time, distilled water is introduced into the micro-nano bubble generator to form a micro-nano gas-liquid dispersion system in the oxidation absorber to catalyze the oxidation and absorption of NO and SO2 gases.

Citation Information

Patent Citations

  • Preparation method of ZnFe2O4 / Ag3PO4 composite photocatalyst

    CN104437573A

  • Method for preparing nanometer MnFe2O4 / graphene composite material

    CN104944474A

  • Ferrite@graphene hydrogel composite material and application of ferrite@graphene hydrogel composite material to electrochemical energy storage field

    CN107705998A

  • Fe3O4 nanoparticle and micro-nano bubble coupled flue gas absorption system and method