Hydro-upgrading catalyst as well as preparation method and application thereof

By pre-adsorbing active metal on the molecular sieve and mixing it with alumina, changing the feeding order to avoid contact with the acid solution, optimizing the catalyst structure, the problem of high frequency of secondary cracking reactions in the prior art is solved, and the 16th day of direct liquefied diesel from coal is improved The alkane number and catalyst life achieve efficient hydrogenation modification effect.

CN118976532AActive Publication Date: 2024-11-19CHINA SHENHUA COAL TO LIQUID & CHEM CO LTD +2

Patent Information

Application Number
CN202411057997.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-19
Estimated Expiration
2044-08-02

AI Technical Summary

Technical Problem

The existing hydrogenation modification catalysts have the problem of high frequency of secondary cracking reactions in improving the ring opening conversion efficiency of aromatic hydrocarbons and cycloalkanes in direct liquefied diesel in coal, and there are fewer modification catalysts for coal-based oil products, especially for The development of catalysts for direct liquefied oil products in coal has not been reported.

Method used

The activated metal is pre-adsorbed on the molecular sieve by immersion, and then mixed with alumina and additives evenly. By changing the feeding order, the molecular sieve is prevented from contacting the acidic solution, the acidic properties and crystal structure of the molecular sieve are maintained, and the active metal with different concentration gradients is passed. Distribution, optimize the pore structure and acidic center distribution of the catalyst to reduce secondary cracking reactions.

Benefits of technology

It significantly improves the selective ring-opening conversion capacity of polycyclic cyclic hydrocarbons in direct liquefied diesel from coal, improves the hexadecane number and yield of diesel, extends the service life of the catalyst, and reduces manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses a hydro-upgrading catalyst as well as a preparation method and application thereof, the preparation method comprises the following steps: (1) preparing a proper amount of active metal solution, impregnating active metal on a molecular sieve by adopting an impregnation method, and then drying to obtain an impregnated molecular sieve for later use; (2) weighing a proper amount of aluminum oxide powder, sesbania powder, citric acid and a nitric acid solution, and uniformly mixing and kneading to obtain a mixed and kneaded material; (3) uniformly mixing the impregnated molecular sieve in the step (1) and the kneaded material in the step (2) to obtain a mixture, kneading and forming on a banded extruder, and then drying and roasting to obtain a carrier; and (4) preparing a certain amount of active metal solution again, impregnating the active metal onto the carrier in the step (3) by adopting an impregnation method, and then drying and roasting to obtain the hydro-upgrading catalyst. According to the invention, the ring-opening conversion efficiency of aromatic hydrocarbon and cycloalkane in the oil product can be improved, the secondary cracking reaction is reduced, and the selectivity of the hydrocracking reaction product is better.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of catalyst technology, in particular to the field of hydro-modification catalysts for naphthenic oil products, and specifically to a hydro-modification catalyst and a preparation method and application thereof. Background Art

[0002] The low-temperature performance of the diesel fraction rich in high cycloalkanes is good, and it is a high-quality low-freezing point diesel, but its cetane number is low and does not meet the national use standards, which affects its performance. According to the investigation, after the polycyclic aromatic hydrocarbons are hydrogenated and saturated, the polycyclic alkane molecules can undergo selective ring-opening reactions on suitable hydrogenation catalysts without secondary cracking and isomerization reactions, generating cycloalkanes with long side chains, which can achieve the goal of significantly improving the cetane number of diesel. Due to the large molecular weight of polycyclic cycloalkanes, the pore size and specific surface area of ​​the hydrogenation catalyst are required to be high. The mesoporous pore size can effectively reduce the diffusion resistance of aromatic macromolecules, can smoothly contact with the active center in the pore, and can diffuse to the catalyst surface in time after the ring-opening reaction, reducing the possibility of secondary cracking. The hydrogenation catalyst is a bifunctional catalyst, which has both a metal component with the activation hydrogenation function and an acidic carrier part with the cracking function. The selection and matching of the two will have an important impact on the activity, selectivity, mechanical strength, thermal stability and service life of the catalyst. Excellent hydrogenation catalysts need to have suitable acidic centers, pore structures and metal active centers. Under the action of high-performance hydrogenation metal catalysts, the ring-opening products can react with active hydrogen as quickly as possible, effectively hindering the secondary cracking of the ring-opening products and improving diesel yield and product performance.

[0003] CN102746894B discloses a selective ring-opening reaction method for aromatic hydrocarbons, in which a hydrogenation reaction is carried out in two reactors connected in series; the material enters the first reactor for deep desulfurization and denitrification reactions, and then undergoes H2 SThe NH3 separation device removes sulfur and nitrogen. When the S content in the material is lower than 50ppm and the N content is lower than 10ppm, the material enters the second reactor for selective ring-opening reaction. The reactor has two reaction beds. The first reaction bed carries out hydrogenation saturation isomerization reaction, and the second reaction bed carries out selective ring-opening reaction. The first reactor selects a traditional hydrogenation desulfurization metal sulfide catalyst, and the bottom of the reactor is filled with CoMo / Al2O3 catalyst; the upper part of the reactor is filled with NiMo / Al2O3 catalyst; the first bed of the second stage reactor adopts a precious metal / molecular sieve catalyst to realize hydrogenation isomerization reaction; then the reaction material enters the precious metal / alumina catalyst of the second bed to realize the ring-opening reaction of the five-membered ring. The catalyst is preferably an Ir / Al2O3 catalyst with strong hydrogenolysis ability. Avoiding the use of an acidic carrier limits the further cracking reaction of the reaction material, thereby ensuring the maximization of the selective ring-opening reaction product. This method can achieve limited shape-selective ring-opening cracking reactions of polycyclic aromatic hydrocarbons and cycloalkanes, thereby improving the cetane number and performance of diesel. However, this method has a complex process flow and high requirements for raw materials. The precious metal catalysts required for the reaction are difficult to prepare and are expensive, making it difficult to meet the needs of large-scale industrial development.

[0004] CN111097487 A provides a catalytic diesel hydrogenation reforming catalyst and its preparation method and application. The preparation of the catalyst comprises the following steps: (1) firstly subjecting the acidic center of the Y molecular sieve to a benzyl quaternary ammonium salt solution impregnation treatment, wherein the benzyl quaternary ammonium salt is selectively distributed in the macropores, and then subjected to oxygen-free carbonization, so that the benzyl quaternary ammonium salt is in situ carbonized in the macropores, thereby blocking the macropore channels, and then subjecting the subsequent sodium ion exchange treatment to selectively shield the acidic center distributed in the small pores of the Y molecular sieve, and finally subjecting the acidic center to a calcination treatment to concentrate the acidic center in the macropore channels; (2) subjecting the modified Y molecular sieve and the oxygen-free carbonization treatment to a calcination treatment; and (3) subjecting the modified Y molecular sieve to a calcination treatment. At least one of aluminum oxide, silicon oxide or amorphous silicon aluminum is mixed evenly, and then a nitric acid aqueous solution with a mass fraction of 20wt% is added to the carrier mixture to make a slurry, which is then extruded and dried and burned; (3) the silicon aluminum carrier is saturated with a solution containing an active metal, and the obtained product is dried and roasted to obtain a hydrogenation catalyst; the modified Y-type molecular sieve provided by the present invention has acid centers mainly distributed in large pores, while a small amount or even no acid centers are distributed in the micropores, which can reduce the hydrocarbon oil molecules entering the micropores and causing secondary cracking reactions on the acid centers. However, this method has a complicated process, and the sodium in the catalyst may react with other elements under high temperature and high pressure conditions to generate salt substances such as NaCl, which will block the microporous structure of the catalyst, thereby reducing the catalytic efficiency.

[0005] CN108452839A patent discloses a method for preparing a mesoporous composite molecular sieve catalyst, which uses molecular sieve (Beta or ZSM-5 / SAPO-5 composite molecular sieve) and MCM-48 mesoporous composite molecular sieve to mix evenly with alumina, and prepares a catalyst carrier after extrusion; VIB and VIII group metals are used as active metals; the active component is loaded on the carrier by an equal volume impregnation or step-by-step impregnation method; the alcohol solution is impregnated, the active component is redispersed, and then dried and roasted to obtain a catalyst product. This method controls the ratio of microporous phase to mesoporous phase in the mesoporous carrier by adding microporous molecular sieves of different masses, so that the acid distribution of the composite carrier can be adjusted, thereby realizing the selective aromatic ring opening of diesel. However, this method has problems such as poor hydrothermal properties of mesoporous MCM-48 molecular sieve, which is not suitable for processing inferior products, and the use of templates is uneconomical and polluting.

[0006] CN200810104303.2 discloses a modified molecular sieve-based noble metal diesel deep hydrogenation and dearomatization catalyst and its preparation method. The method comprises the following steps: (1) preparing HY molecular sieve by ion exchange; (2) performing dealumination and siliconization modification on the HY molecular sieve to prepare a carrier; (3) impregnating with a Group VIII noble metal salt solution, drying, calcining and activating to obtain a catalyst. The catalyst adopts an active component system of noble metal plus an auxiliary agent, and although it has good ring-opening activity, it has weak resistance to heteroatoms such as S and N in the raw materials.

[0007] The current hydrogenation catalyst is mainly made of molecular sieves, mainly including USY, Beta or ZSM-5 / SAPO-5 molecular sieves or composite molecular sieves, which are evenly mixed with traditional γ-Al2O3, and then a certain amount of nitric acid is added as a binder. The powder is kneaded and formed, and then dried and calcined as a catalyst carrier. In this process, the addition of inorganic acid has a great influence on the molecular sieve. The inorganic acid and the aluminum element of the molecular sieve act to destroy the pore structure and crystallinity of the molecular sieve, and affect the acid properties and hydrothermal stability of the molecular sieve. In addition, the acid added to the extrusion causes the carrier to produce NOx during the calcination process, forming air pollution, which does not meet the requirements of green production. At present, the γ-Al2O3 used in industrial production is mainly SB powder, which is expensive and has a small pore volume, which is not conducive to the diffusion of macromolecules in the pores. The catalyst prepared using SB powder has a large bulk density. In the same reactor, the catalyst with a large density is also used in large amounts, and the economic efficiency is low.

[0008] In addition, the hydro-reforming catalysts currently on the market are mainly designed and prepared for petroleum-based oil products, and there are few hydro-reforming catalysts for coal-based oil products, especially for coal direct liquefaction oil products. By developing hydro-reforming catalysts for coal-based oil products, the selective ring opening of aromatics and cycloalkanes can be achieved to generate cycloalkanes with long side chains, which can effectively improve the cetane number of coal-based diesel and the viscosity-temperature performance of cycloalkane oil products. Summary of the invention

[0009] The purpose of the present invention is to provide a hydrogenation reforming catalyst and its preparation method and application, so as to improve the ring-opening conversion efficiency of aromatics and cycloalkanes, especially cycloalkanes with two or more rings, in coal direct liquefaction diesel and reduce the occurrence of secondary cracking reactions.

[0010] To achieve one aspect of the above-mentioned invention object, the present invention adopts the following technical solution:

[0011] A method for preparing a hydrogenation catalyst comprises the following steps:

[0012] (1) preparing an appropriate amount of active metal solution and impregnating the active metal on the molecular sieve by an impregnation method, and then drying to obtain an impregnated molecular sieve for standby use;

[0013] (2) mixing and kneading the ingredients including pseudo-boehmite, sesbania powder, citric acid and nitric acid solution to obtain a mixed material;

[0014] (3) mixing the impregnated molecular sieve in step (1) and the kneaded material in step (2) to obtain a mixed material, kneading and shaping the mixed material on an extruder, and then drying and calcining the mixed material to obtain a carrier;

[0015] (4) preparing a certain amount of active metal solution again, and impregnating the active metal onto the carrier of step (3) by an impregnation method, and then drying and calcining to obtain the hydrogenation reforming catalyst.

[0016] In step (1) of the present invention, the active metal solution is impregnated onto the molecular sieve so that a certain amount of active metal can be pre-adsorbed on the molecular sieve. The molecular sieve used can be a commonly used molecular sieve for preparing supported hydrogenation catalysts in the art; in some embodiments, the molecular sieve is selected from one or more of USY, HY, REY, Beta, SAPO-5 and ZSM-5 molecular sieves.

[0017] In a preferred embodiment, the active metal impregnated in step (1) accounts for less than 50 wt% of the total active metal in the hydroreforming catalyst, such as 10%, 20 wt%, 30 wt% or 40 wt%, preferably 10-30 wt%.

[0018] In the present invention, the active metal used to prepare the active metal solution can be an active metal commonly used in oil hydrogenation and reforming catalysts well known in the art, for example, selected from Group VIII and / or Group VI elements in the periodic table; preferably, the Group VIII active metal is Ni and / or Co, and the Group VI active metal is W and / or Mo.

[0019] In step (2) of the present invention, pseudo-boehmite as a precursor of alumina as a part of the carrier is kneaded with sesbania powder, citric acid and nitric acid solution to obtain a mixture, thereby avoiding direct contact between the molecular sieve as another part of the carrier and nitric acid, so as to maintain the crystal structure, pore properties and acid properties of the molecular sieve.

[0020] In a preferred embodiment, the mixed material also contains auxiliary elements, which are one or more of Si, B, Zr, Ti, La and Ce; preferably, the amount of the auxiliary elements calculated as their oxides is 0.1-8wt% of the total amount of the molecular sieve and pseudo-boehmite, such as 0.5wt%, 1wt%, 3wt%, 5wt% or 7wt%; studies have found that the added auxiliary elements can subsequently react with alumina to reduce L acid, increase some B acid, reduce the amount of carbon deposits on the catalyst, and extend the service life of the catalyst.

[0021] In step (3) of the present invention, the impregnated molecular sieve is mixed with the kneading material, kneaded and formed on an extruder, and then dried and calcined to obtain a carrier. It is understood in the art that after calcination, the pseudo-boehmite is converted into alumina so as to be used as a carrier; in a preferred embodiment, in the carrier, the mass ratio of the molecular sieve to the alumina obtained by calcining and decomposing the pseudo-boehmite is 1:9-3:2, such as 1:8, 1:6, 1:5, 1:3, 1:2 or 1:1, preferably 1:4-2:3.

[0022] In some embodiments, in order to ensure good kneading and extrusion performance of the mixture, the amount of the sesbania powder is 0.5%-10wt%, preferably 1-5wt%, such as 2wt%, 3wt% or 4wt%, based on the total amount of the molecular sieve and the pseudo-boehmite. That is, when the total amount of the molecular sieve and the pseudo-boehmite is 100 parts by weight, the amount of the sesbania powder can be 0.5-10 parts by weight, which is easily understood in the art and will not be repeated here; the amount of citric acid is 0.5%-10wt%, preferably 1-5wt%. 1-5wt%, such as 2wt%, 3wt% or 4wt%; the concentration of the nitric acid solution is 0.2-1mol / L, and the amount is 0.5-2wt%, preferably 1-1.5wt%, such as 1.2wt%, 1.3wt% or 1.4wt%; when an auxiliary agent is added, the precursor of the auxiliary agent element (such as boric acid) is dissolved in the nitric acid solution so as to be evenly mixed with the remaining ingredients, and the amount of the auxiliary agent element calculated as its oxide is 0.5-5wt% of the total amount of the USY molecular sieve and pseudo-boehmite.

[0023] In step (4) of the present invention, a certain amount of active metal solution is prepared again, and the active metal is impregnated onto the carrier by an impregnation method, and then dried and calcined to obtain the hydrogenation reforming catalyst; through two impregnations, the active metal amounts of the molecular sieve and the alumina have different concentration gradients.

[0024] Of course, it is understood in the art that the active metal solution can also be prepared once and used in steps (1) and (4) respectively, which should be regarded as equivalent to the present invention.

[0025] In a preferred embodiment, in the above step (4), the active metals are calculated in the form of their oxides. In the hydroreforming catalyst, the Group VIII active metals account for 1-10 wt%, preferably 3-5 wt%, and the Group VI active metals account for 10-40 wt%, preferably 15-30 wt%.

[0026] In a preferred embodiment, the Group VIII active metal impregnated in step (4) accounts for 50-90wt%, such as 60wt%, 70wt% or 80wt% of the total amount of Group VIII active metals in the hydroreforming catalyst, and the Group VI active metal impregnated in step (4) accounts for 50-90wt%, such as 60wt%, 70wt% or 80wt% of the total amount of Group VI active metals in the hydroreforming catalyst.

[0027] In a preferred embodiment, the active metal of Group VIII is Ni and the active metal of Group VI is W. The active metal solution in the above steps (1) and (4) is prepared as follows: about 70% of deionized water is added to a beaker, and after heating to 40-50°C, citric acid and phosphoric acid are added, and after stirring evenly, basic nickel carbonate is added. After the basic nickel carbonate is dissolved, ammonium metatungstate is added. After the ammonium metatungstate is completely dissolved, the volume is fixed to the required volume. Preferably, when preparing the active metal solution, the mass ratio of the citric acid added to the nickel oxide is (0.1-5.0):1, preferably (0.5-2.0):1, such as 1:1; the amount of phosphoric acid added is 0.5%-5.0% of the mass of the hydrogenation catalyst, preferably 1.0%-3.0%, calculated as phosphorus oxide.

[0028] In the present invention, the impregnation method may be an equal volume impregnation method to facilitate control of the impregnation load. Of course, it is understood in the art that other impregnation methods may also be used, which are all well known in the art and will not be described in detail here.

[0029] In addition, the present invention also involves drying and calcining of related materials, which are conventional treatment methods for preparing supported hydrogenation catalysts in the art and are well known in the art. For example, the drying can be performed at 80-120° C. for 6-12 hours; for example, the calcination can be performed at 500-550° C. for 3-6 hours.

[0030] To achieve another aspect of the above-mentioned object of the invention, the present invention also provides a hydrogenation reforming catalyst prepared according to the above-mentioned preparation method.

[0031] In some embodiments, the specific surface area of ​​the hydro-reforming catalyst is 200-400m 2 / g, pore volume is 0.2-0.5cm 3 / g, and the average pore size is 5-15nm; it is understood in the art that good porous properties are beneficial to reducing the diffusion resistance of molecules in the pores, reducing the density of the catalyst, and reducing the manufacturing cost.

[0032] To achieve another aspect of the above-mentioned purpose of the invention, the present invention also provides the use of the hydro-modification catalyst in the hydro-modification of oil products, wherein the oil products are oil products containing aromatic hydrocarbons and cycloalkanes, preferably aromatic compounds containing benzene, naphthalene, phenanthrene, coal tar, coal direct liquefaction oil, and cycloalkane oil.

[0033] In the present invention, unless otherwise specified, all percentages or percents involved are mass percentages or mass percents.

[0034] Compared with the prior art, the present invention has the following advantages:

[0035] The present invention innovatively changes the order of adding materials, avoids the contact between the molecular sieve and the acidic solution, is beneficial to maintaining the acid properties and crystal structure of the molecular sieve, is beneficial to the hydrogenation and modification performance of the catalyst, and can extend the service life of the catalyst. It is a new type of hydrogenation and modification carrier preparation technology. In addition, the present invention adopts different concentration gradients for the active metal content of the molecular sieve and alumina, so that the active metal density near the acid center of the catalyst is higher; before mixing, the molecular sieve is first impregnated with a part of the active metal solution, and after drying, it is evenly mixed with the alumina, and citric acid, field sesbania powder and the like are added to knead and shape, and a part of the active metal carrier is obtained after drying and roasting; the remaining metal solution is then impregnated on the above-mentioned carrier to obtain a catalyst with different metal concentration gradients, which is beneficial for the cracked molecules to quickly contact the metal center for hydrogenation and stabilization, avoid further cracking, reduce the occurrence of secondary cracking reactions, and thus greatly improve the catalyst selectivity; the hydrogenation and modification catalyst of the present invention should have the characteristics that the acid center of the carrier itself matches the hydrogenation / dehydrogenation center strength of the catalyst, and the distance between the two centers is as close as possible; in addition, through the action of the auxiliary element and the alumina, the L acid can be reduced, and part of the B acid can be increased, so that the carbon deposition of the catalyst can be reduced and the service life of the catalyst can be extended.

[0036] The catalyst prepared by the method of the present invention has excellent selective ring-opening conversion ability of polycyclic cycloalkanes, can greatly improve the cetane number of coal direct liquefaction diesel products, and at the same time, has a high diesel yield, and has broad application prospects in the process of coal-based oil hydrogenation and upgrading reactions. DETAILED DESCRIPTION

[0037] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.

[0038] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values, such as values ​​of ±10% of the endpoint values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. In the absence of conflict, the embodiments in this application and the features in the embodiments can be combined with each other.

[0039] It should be noted that the terms "include" and "have" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or apparatus comprising a series of steps or units is not necessarily limited to those steps or units explicitly listed, but may include other steps or units not explicitly listed or inherent to these processes, methods, products or apparatus.

[0040] In the following examples / comparative examples, unless otherwise specified, all reagents used were of analytical grade.

[0041] Example 1

[0042] This embodiment provides a method for preparing a hydrogenation catalyst, which comprises the following steps:

[0043] (1) Take an appropriate amount of deionized water, heat it to 50°C, weigh citric acid and phosphoric acid, add them to the deionized water, stir for 0.5h, add basic nickel carbonate solid, add ammonium metatungstate after the basic nickel carbonate is dissolved, and after the ammonium metatungstate is completely dissolved, adjust the volume to the required volume of active metal solution for standby use; wherein the mass ratio of citric acid to nickel oxide is 0.5:1, and the amount of phosphoric acid added is 1% of the mass of the hydrogenation catalyst calculated as phosphorus oxide; weigh an appropriate amount of USY molecular sieve powder, pour the prepared solution into the molecular sieve and impregnate it evenly, and dry it at 80°C for 6h;

[0044] (2) Weigh appropriate amounts of pseudo-boehmite powder (hereinafter referred to as PB powder), sesbania powder and citric acid, mix them evenly, then add an appropriate amount of nitric acid solution with a nitric acid concentration of 0.3 mol / L, to which boric acid is also added, and knead them evenly after they are completely dissolved; wherein the mass ratio of alumina obtained by decomposing pseudo-boehmite to USY molecular sieve is 4:1; and based on the total amount of the USY molecular sieve and pseudo-boehmite, the amount of sesbania powder is 1%, the amount of citric acid is 1%, the amount of nitric acid solution is 1%, and the amount of auxiliary boron calculated as boron oxide is 1%;

[0045] (3) The molecular sieve impregnated with metal and dried in step (1) is mixed evenly with the mixed material kneaded in step (2), and kneaded on an extruder to form a carrier, which is dried and calcined to obtain a carrier named Z-1, wherein the amount of nickel oxide and tungsten oxide accounts for 10% of the total amount of nickel oxide in the catalyst, and the amount of tungsten oxide accounts for 10% of the total amount of tungsten oxide in the catalyst. The drying temperature is 80°C and the time is 6 hours, and the calcination temperature is 500°C and the time is 6 hours;

[0046] (4) Prepare the remaining active metal solution in the same manner as in step (1), and impregnate it into the above-mentioned carrier. After drying and calcining, a catalyst is obtained, named C-1; wherein the drying temperature is 80°C, the time is 6 hours, and the calcining temperature is 500°C, the time is 6 hours; in the catalyst, the mass fraction of nickel oxide is 3%, and the mass fraction of tungsten oxide is 22.5%

[0047] Example 2

[0048] (1) Take an appropriate amount of deionized water, heat it to 50°C, weigh citric acid and phosphoric acid, add them to the deionized water, stir for 0.5h, add basic nickel carbonate solid, add ammonium metatungstate after the basic nickel carbonate is dissolved, and after the ammonium metatungstate is completely dissolved, adjust the volume to the required volume of active metal solution for standby use; wherein the mass ratio of citric acid to nickel oxide is 1:1, and the amount of phosphoric acid added is 1.2% of the mass of the hydrogenation catalyst calculated as phosphorus oxide; weigh an appropriate amount of USY molecular sieve powder, pour the prepared solution into the molecular sieve and impregnate it evenly, and dry it at 100°C for 4h;

[0049] (2) Weigh appropriate amounts of PB powder, sesbania powder and citric acid, mix them evenly, then add appropriate amounts of nitric acid solution with a nitric acid concentration of 0.5 mol / L, to which boric acid is also added, and knead them evenly after they are completely dissolved; wherein the mass ratio of alumina obtained by decomposing pseudo-boehmite to USY molecular sieve is 7:3; and based on the total amount of the USY molecular sieve and pseudo-boehmite, the amount of sesbania powder is 2%, the amount of citric acid is 2%; the amount of nitric acid solution is 1.1%; and the amount of auxiliary boron calculated as boron oxide is 2%;

[0050] (3) The molecular sieve impregnated with metal and dried in step (1) is mixed evenly with the mixed material kneaded in step (2), and kneaded on an extruder to form a carrier, which is dried and calcined to obtain a carrier named Z-2, wherein the amount of nickel oxide and tungsten oxide accounts for 20% of the total amount of nickel oxide in the catalyst, and the amount of tungsten oxide accounts for 20% of the total amount of tungsten oxide in the catalyst. The drying temperature is 100°C and the time is 4 hours, and the calcination temperature is 550°C and the time is 4 hours;

[0051] (4) Prepare the remaining active metal solution in the same manner as in step (1), and impregnate it into the above-mentioned carrier. After drying and calcining, a catalyst named C-2 is obtained; wherein the drying temperature is 100° C. and the time is 4 h, and the calcining temperature is 550° C. and the time is 4 h. In the catalyst, the mass fraction of nickel oxide is 3%, and the mass fraction of tungsten oxide is 22.5%.

[0052] Example 3

[0053] (1) Take an appropriate amount of deionized water, heat it to 50°C, weigh citric acid and phosphoric acid, add them to the deionized water, stir for 0.5h, add basic nickel carbonate solid, add ammonium metatungstate after the basic nickel carbonate is dissolved, and after the ammonium metatungstate is completely dissolved, adjust the volume to the required volume of active metal solution for standby use; wherein the mass ratio of citric acid to nickel oxide is 1.5:1, and the amount of phosphoric acid added is 1.2% of the mass of the hydrogenation catalyst calculated as phosphorus oxide; weigh an appropriate amount of USY molecular sieve powder, pour the prepared solution into the molecular sieve and impregnate it evenly, and dry it at 120°C for 3h;

[0054] (2) Weigh appropriate amounts of PB powder, sesbania powder and citric acid, mix them evenly, then add an appropriate amount of nitric acid solution with a nitric acid concentration of 0.5 mol / L, to which boric acid is also added, and knead them evenly after they are completely dissolved; wherein the mass ratio of alumina obtained by decomposing pseudo-boehmite to USY molecular sieve is 3:2; and based on the total amount of the USY molecular sieve and pseudo-boehmite, the amount of sesbania powder is 3%, the amount of citric acid is 3%; the amount of nitric acid solution is 1.2%; and the amount of auxiliary boron calculated as boron oxide is 3%;

[0055] (3) The molecular sieve impregnated with metal and dried in step (1) is mixed evenly with the mixed material kneaded in step (2), and kneaded on an extruder to form a carrier, which is dried and calcined to obtain a carrier named Z-3, wherein the amount of nickel oxide and tungsten oxide accounts for 20% of the total amount of nickel oxide in the catalyst, and the amount of tungsten oxide accounts for 20% of the total amount of tungsten oxide in the catalyst. The drying temperature is 120°C and the time is 3 hours, and the calcination temperature is 550°C and the time is 3 hours;

[0056] (4) The remaining active metal solution is prepared in the same manner as in step (1), and impregnated into the above-mentioned carrier. After drying and calcination, a catalyst is obtained, which is named C-3; wherein the drying temperature is 120° C. and the time is 3 h, and the calcination temperature is 550° C. and the time is 3 h; in the catalyst, the mass fraction of nickel oxide is 3%, and the mass fraction of tungsten oxide is 22.5%.

[0057] Example 4

[0058] (1) Take an appropriate amount of deionized water, heat it to 50°C, weigh citric acid and phosphoric acid, add them to the deionized water, stir for 0.5h, add basic nickel carbonate solid, add ammonium metatungstate after the basic nickel carbonate is dissolved, and after the ammonium metatungstate is completely dissolved, adjust the volume to the required volume of active metal solution for standby use; wherein the mass ratio of citric acid to nickel oxide is 1.5:1, and the amount of phosphoric acid added is 1.2% of the mass of the hydrogenation catalyst calculated as phosphorus oxide; weigh an appropriate amount of USY molecular sieve powder, pour the prepared solution into the molecular sieve and impregnate it evenly, and dry it at 120°C for 3h;

[0059] (2) Weigh appropriate amounts of PB powder, sesbania powder and citric acid, mix them evenly, then add an appropriate amount of nitric acid solution with a nitric acid concentration of 0.6 mol / L, to which boric acid is also added, and knead them evenly after they are completely dissolved; wherein the mass ratio of alumina obtained by decomposing pseudo-boehmite to USY molecular sieve is 3:2; and based on the total amount of the USY molecular sieve and pseudo-boehmite, the amount of sesbania powder is 3%, the amount of citric acid is 3%; the amount of nitric acid solution is 1.1%; and the amount of auxiliary boron in terms of boron oxide is 3%;

[0060] (3) The molecular sieve impregnated with metal and dried in step (1) is mixed evenly with the mixed material kneaded in step (2), and kneaded on an extruder to form a carrier, which is dried and calcined to obtain a carrier named Z-4, wherein the amount of nickel oxide and tungsten oxide accounts for 30% of the total amount of nickel oxide in the catalyst, and the amount of tungsten oxide accounts for 30% of the total amount of tungsten oxide in the catalyst. The drying temperature is 120°C and the time is 3 hours, and the calcination temperature is 550°C and the time is 3 hours;

[0061] (4) The remaining active metal solution is prepared in the same manner as in step (1), and impregnated into the above-mentioned carrier. After drying and calcination, a catalyst is obtained, which is named C-4; wherein the drying temperature is 120° C. and the time is 3 h, and the calcination temperature is 550° C. and the time is 3 h; in the catalyst, the mass fraction of nickel oxide is 3%, and the mass fraction of tungsten oxide is 22.5%.

[0062] Example 5

[0063] The difference from Example 3 is that in step (1), the molecular sieve used is changed to a mixed molecular sieve of USY and β, wherein the mass ratio of USY to β molecular sieve is 7:3. The rest is the same as Example 3. The obtained catalyst is named C-5.

[0064] Example 6

[0065] The difference between Example 6 and Example 5 is that no auxiliary boron element is added in step (2). The obtained catalyst is named C-6.

[0066] Comparative Example 1:

[0067] The difference from Example 2 is that: in step (2), the impregnated dried molecular sieve in step (1) is directly mixed with PB powder, sesbania powder and citric acid, and then an appropriate amount of 0.5 mol / L nitric acid solution is added to prepare a kneaded material; in step (3), the kneaded material is directly kneaded and formed on an extruder. The rest is the same as Example 3. The obtained catalyst is named D-1.

[0068] Comparative Example 2:

[0069] The difference from Comparative Example 1 is that in step (1), the USY molecular sieve is no longer impregnated with the active metal solution prepared in step (1); in step (2), the unimpregnated USY molecular sieve is directly mixed with PB powder, sesbania powder and citric acid; in step (3), the obtained carrier is further impregnated with the active metal solution prepared in step (1) and dried. The rest is the same as Comparative Example 1. The obtained catalyst is named D-2.

[0070] Comparative Example 3

[0071] The difference from Example 5 is that: in step (1), the USY and β molecular sieves are no longer impregnated with the active metal solution prepared in step (1); in step (2), the unimpregnated USY molecular sieve is directly mixed with PB powder, sesbania powder and citric acid, and then an appropriate amount of nitric acid solution with a concentration of XX is added to prepare a kneaded material; in step (3), the above-mentioned kneaded material is directly kneaded and formed on an extruder; and in step (3), the obtained carrier is further impregnated with the active metal solution prepared in step (1) and dried. The rest is the same as in Example 5. The obtained catalyst is named D-3.

[0072] Table 1 Comparison of composition and physicochemical properties of examples and comparative examples

[0073] Catalyst No. C-1 C-2 C-3 C-4 C-5 C-6 D-1 D-2 D-3 PB:(USY+β) 4:1 7:3 3:2 3:2 3:2 3:2 3:2 3:2 3:2 USY: β - - - - 7:3 7:3 7:3 7:3 7:3 NiO-1, wt% 10 20 20 30 20 20 20 - - <![CDATA[WO3-1,wt%]]> 10 20 20 30 20 20 20 - - NiO-2, wt% 3 3 3 3 3 3 3 3 3 <![CDATA[WO3-2,wt%]]> 22.5 22.5 22.5 22.5 22.5 22.5 22.5 22.5 22.5 <![CDATA[Specific surface area, m 2 / g]]> 293 300 308 302 325 325 310 313 330 <![CDATA[Pore volume, cm 3 / g]]> 0.32 0.34 0.37 0.32 0.34 0.34 0.33 0.32 0.32 Average pore size, nm 8.8 8.6 8.5 8.6 8.2 8.0 8.4 8.4 8.2

[0074] Note: NiO-1 and WO3-1 are the percentage of active metal mass in the molecular sieve to the total metal mass; NiO-2 and WO3-2 are the mass fraction of active metal mass in the catalyst.

[0075] Table 2 Comparison of acid properties of catalysts in Examples and Comparative Examples

[0076] catalyst Medium strong acid strong acid Medium acid / strong acid C-1 2250.6 1800.5 1.25 C-2 2561.2 1883.2 1.36 C-3 2625.0 1750 1.50 C-4 2638.4 1845 1.43 C-5 2805.0 1700 1.65 C-6 2680 1675 1.60 D-1 2171.7 1905 1.14 D-2 2021.3 1925 1.05 D-3 2301.6 1918 1.20

[0077] It can be seen from Table 2 that by changing the order of adding nitric acid and avoiding direct contact of molecular sieve with nitric acid, the amount of medium-strong acid in the catalyst increases, the amount of strong acid decreases, and the ratio of medium-strong acid / strong acid increases, the effect of catalyst ring opening without breaking can be improved.

[0078] The above catalyst was used to carry out oil product hydrogenation reforming reaction (reaction temperature 350°C, reaction pressure 13MPa, reaction space velocity 2.5h -1 Under the condition of hydrogen-to-oil ratio of 800, the relevant oil properties are shown in Table 3.

[0079] Table 3 Results of coal liquefaction oil hydro-reforming reaction with different catalysts under reaction condition 1

[0080]

[0081]

[0082] From the comparison of the above embodiments / comparative examples, it can be seen that the catalyst hydrogenation performance can be improved by avoiding direct contact between the molecular sieve and the acidic solution and changing the active metal concentration of the molecular sieve and the PB powder; in addition, 20% of the active metal solution is first impregnated on the molecular sieve, and the catalyst with PB (wt%): (USY + β) (wt%) = 3:2, among which the C-5 catalyst with USY (wt%): β (wt%) = 7:3 has the best reaction performance, can achieve ring-opening and uninterrupted chain performance, and significantly improves the cetane number of the raw material.

Claims

1. A method for preparing a hydrogenation catalyst, comprising the following steps: (1) preparing an appropriate amount of active metal solution and impregnating the active metal on the molecular sieve by an impregnation method, and then drying to obtain an impregnated molecular sieve for standby use; (2) kneading the ingredients including pseudo-boehmite, sesbania powder, citric acid and nitric acid solution uniformly to obtain a kneaded material; (3) mixing the impregnated molecular sieve in step (1) and the kneaded material in step (2) to obtain a mixed material, kneading and shaping the mixed material on an extruder, and then drying and calcining the mixed material to obtain a carrier; (4) preparing a certain amount of active metal solution again, and impregnating the active metal onto the carrier of step (3) by an impregnation method, and then drying and calcining to obtain the hydrogenation reforming catalyst.

2. The preparation method according to claim 1, characterized in that: The active metal impregnated in step (1) accounts for less than 50% of the total amount of active metal in the hydroreforming catalyst, preferably 10-30%.

3. The preparation method according to claim 2, characterized in that: The mixed material further contains auxiliary elements, and the auxiliary elements are one or more of Si, B, Zr, Ti, La and Ce; Preferably, the amount of the auxiliary element calculated as its oxide is 0.1-8 wt % of the total amount of the molecular sieve and pseudo-boehmite.

4. The preparation method according to claim 3, characterized in that: In the above step (1), the molecular sieve is selected from one or more of USY, HY, REY, Beta, SAPO-5 and ZSM-5 molecular sieves; in step (1) and step (4), the active metal is selected from Group VIII and / or Group VI elements in the periodic table, wherein the Group VIII active metal is preferably Ni and / or Co, and the Group VI active metal is preferably W and / or Mo.

5. The preparation method according to claim 4, characterized in that: The active metal is calculated in the form of its oxide. In the hydroreforming catalyst, the Group VIII active metal accounts for 1-10wt%, preferably 3-5wt%, and the Group VI active metal accounts for 10-40wt%, preferably 15-30%; The Group VIII active metal impregnated in step (4) accounts for 50-90% of the total amount of the Group VIII active metal in the hydroreforming catalyst, and the Group VI active metal impregnated in step (4) accounts for 50-90% of the total amount of the Group VI active metal in the hydroreforming catalyst.

6. The preparation method according to claim 5, characterized in that: In the carrier of the above step (3), the mass ratio of the molecular sieve to the alumina obtained by calcining and decomposing pseudo-boehmite is 1:9-3:2, preferably 1:4-2:3; and based on the total amount of the molecular sieve and pseudo-boehmite, the amount of the sesbania powder is 0.5%-10wt%, preferably 1-5wt%, the amount of the citric acid is 0.5%-10wt%, preferably 1-5wt%, the nitric acid concentration of the nitric acid solution is 0.2-1mol / L, and the amount is 0.5-2wt%, preferably 1-1.5wt%; the precursor of the auxiliary element is dissolved in the nitric acid solution so as to be evenly mixed with the remaining ingredients, and the amount of the auxiliary element in terms of its oxide is 0.5-5wt% of the total amount of the USY molecular sieve and pseudo-boehmite.

7. The preparation method according to claim 6, characterized in that: In the active metal solution in the above steps (1) and (4), the Group VIII active metal is Ni and the Group VI active metal is W. The preparation method is as follows: add deionized water to a beaker, heat it to 40-50°C, add citric acid and phosphoric acid, stir evenly, add basic nickel carbonate, add ammonium metatungstate after the basic nickel carbonate is dissolved, and adjust the volume to the required volume after the ammonium metatungstate is completely dissolved.

8. The preparation method according to claim 7, characterized in that: When preparing the active metal solution, the mass ratio of the citric acid added to the nickel oxide is (0.1-5.0):1, preferably (0.5-2.0):1; the mass of the phosphoric acid added is 0.5%-5.0%, preferably 1.0%-3.0%, of the mass of the hydrogenation catalyst, calculated as phosphorus oxide.

9. The preparation method according to claim 8, characterized in that: The impregnation method is an equal volume impregnation method; the drying is drying at 80-120° C. for 6-12 hours; and the calcination is calcining at 500-550° C. for 3-6 hours.

10. The hydro-reforming catalyst prepared according to any one of claims 1 to 9; preferably, the specific surface area of ​​the catalyst is 200-400m 2 / g, pore volume is 0.2-0.5cm 3 / g, and the average pore size is 5-15nm.

11. The use of the hydro-upgrading catalyst according to claim 10 in oil hydro-upgrading, wherein: The oil product is an oil product containing aromatic hydrocarbons and cycloalkane, preferably an aromatic compound containing benzene, naphthalene, phenanthrene, coal tar, coal direct liquefaction oil and cycloalkane oil.

Citation Information

Patent Citations

  • Hydrogenating and pour point depressing catalyst and its preparing method

    CN101143333A

  • Preparation of catalyst catalyzing diesel hydro-conversion, and hydrogenation process

    CN105618111A

  • Seed crystal-assisted preparation method of C8 aromatic hydrocarbon isomerization catalyst

    CN110496643A

  • Preparation method of diesel oil hydro-upgrading catalyst

    CN111905799A

  • Preparation method of hydrodesulfurization and dearomatization catalyst

    CN113522352A

Cited By

  • Composite modified catalyst for preparing clean fuel by heavy oil hydrocracking and preparation method of composite modified catalyst

    CN121266620A