High-adhesiveness electrostatic powder spraying process for iron handicrafts
Through the high adhesion electrostatic powder spraying process of iron crafts, including surface treatment, pretreatment, spray treatment and powder curing treatment, the problem of coating falling off due to bumps and improve adhesion and mechanical properties.
Patent Information
- Application Number
- CN202411041133.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
AI Technical Summary
Some finished products have cracked the coating due to bumps, and the coating has no adhesion at all, and there is a large area of falling off.
The high adhesion electrostatic powder spraying process of iron crafts is adopted, including surface treatment, pretreatment, spray treatment and powder curing treatment steps. The surface treatment is sand-milled and cleaned, the pretreatment is preheated using conductive fluid and oven, the spraying treatment controls the thickness of the powder layer, and the powder curing treatment is heated, insulated and cooled by oven baking.
Improves the adhesion of the coating, prevents the coating from falling off, and ensures the mechanical properties and surface quality of the profile.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of powder spraying technology, and in particular to a high-adhesion electrostatic powder spraying technology for iron handicrafts. Background Art
[0002] Metal profiles are widely used in the construction industry due to their excellent durability, decorativeness and processability. Aluminum profiles account for more than 80% of the metal profile usage due to their excellent processability and light weight. In particular, aluminum building materials sprayed with powder coatings have significantly lower water and air pollution and energy consumption compared to anodizing and electrophoretic coating surface treatment methods.
[0003] However, some finished products now have cracked coatings due to bumps, and the coatings have no adhesion at all, with large areas of peeling off. Summary of the invention
[0004] The purpose of the present invention is to provide a high-adhesion electrostatic powder spraying process for iron crafts to solve the problem that some finished products in the above-mentioned background technology currently have cracks in the coating due to bumps, the coating has no adhesion at all, and there is a large area of shedding.
[0005] In order to achieve the above object, the present invention provides the following technical solution: a high-adhesion electrostatic powder spraying process for iron crafts, comprising the following steps: Step 1: Surface treatment: Use a grinding wheel grinder to sand the outer surface of the craft to improve the surface flatness, then use a high-pressure blower to blow away the dust on the outer surface of the craft, then use a cleaning agent to rinse the outer surface of the craft and dry it in the sun; Step 2: Pretreatment: Evenly apply conductive liquid on the outer surface of the craft, and then put it into the oven for preheating; Step 3: Spraying: Use an electrostatic spraying device to evenly spray the powder onto the outer surface of the craft; Step 4: Powder curing treatment: Put the handicraft sprayed with powder into an oven for baking. The baking process needs to go through three stages: heating, heat preservation, and cooling. After cooling, the desired handicraft can be obtained.
[0006] The technical problem to be solved by the present invention can also be achieved by the following technical solution, wherein the cleaning agent in step 1 is acetone or anhydrous ethanol solution.
[0007] The technical problem to be solved by the present invention can also be achieved by the following technical solution: the preheating temperature of the oven in step 2 is 80° C., and the preheating time is 15 minutes.
[0008] The technical problem to be solved by the present invention can also be achieved by the following technical solution. The pretreatment in step 2 can also be: after mixing the conductive liquid and ethanol in a certain proportion, evenly brushing it on the outer surface of the handicraft, and then drying it.
[0009] The technical problem to be solved by the present invention can also be achieved by the following technical solution, wherein the ratio of the conductive liquid to ethanol is 1:50.
[0010] The technical problem to be solved by the present invention can also be achieved by the following technical solution. In the spraying process described in step 3, the thickness of the powder layer should be well controlled, and the thickness of the powder layer is preferably controlled at 60-80um.
[0011] The technical problem to be solved by the present invention can also be achieved by the following technical solution. In step 4, the baking temperature and time of the oven should be controlled. The baking time is more preferably 18-22 minutes, and the baking temperature is more preferably 180-220°C.
[0012] In the above technical solution, the technical effects and advantages provided by the present invention are: The key to the quality of the spray profile surface lies in the control of various process parameters during the spraying process, especially the amount of powder output and the uniformity of powder distribution. In order to ensure the coating quality of the profile, the thickness of the powder layer must be controlled during the powder spraying process. If the powder layer is too thin, the bottom will be exposed and particles will be generated on the surface. If the powder layer is too thick, the coating will produce orange peel, pinholes, flow marks, etc., and the mechanical properties of the profile will also decrease. DETAILED DESCRIPTION
[0013] In order to enable those skilled in the art to better understand the technical solution of the present invention, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments.
[0014] A high-adhesion electrostatic powder spraying process for iron crafts, comprising the following steps: Step 1: Surface treatment: Use a grinding wheel grinder to sand the outer surface of the craft to improve the surface flatness, then use a high-pressure hair dryer to blow away the dust on the outer surface of the craft, then use acetone or anhydrous ethanol solution to rinse the outer surface of the craft, and dry it in the sun.
[0015] Step 2: Pretreatment: Evenly apply conductive liquid on the outer surface of the craft, and then put it into the oven for preheating. The preheating temperature of the oven is 80°C and the preheating time is 15 minutes.
[0016] The pretreatment in step 2 may also be to mix the conductive liquid and ethanol in a ratio of 1:50, evenly apply the mixture on the outer surface of the handicraft, and then air-dry the mixture.
[0017] Step 3: Spraying: Use an electrostatic spraying device to evenly spray the powder onto the outer surface of the craft. During the spraying process, the thickness of the powder layer should be well controlled. It is more appropriate to control the thickness of the powder layer at 60-80um.
[0018] Step 4: Powder curing treatment: Put the handicraft sprayed with powder into the oven for baking. The baking process needs to go through three stages: heating, heat preservation and cooling. The baking temperature and time of the oven must be controlled. The baking time is more suitable for 18-22 minutes and the baking temperature is more suitable for 180-220℃. After cooling, the desired handicraft can be obtained. Example
[0019] Use a grinding wheel grinder to sand the outer surface of the craft to improve the surface flatness, then use a high-pressure hair dryer to blow away the dust on the outer surface of the craft, then use acetone or anhydrous ethanol solution to rinse the outer surface of the craft, and dry it. Apply the conductive liquid evenly on the outer surface of the craft, and then put it in the oven for preheating. The preheating temperature of the oven is 80℃, and the preheating time is 15min. Use an electrostatic spraying device to evenly spray the powder on the outer surface of the craft. During the spraying process, the thickness of the powder layer should be controlled. The thickness of the powder layer should be controlled at 60-80um. Put the craft sprayed with powder into the oven for baking. The baking process needs to go through three stages of heating, heat preservation, and cooling. The baking temperature and time of the oven should be controlled. The baking time is more suitable for 18-22min and the baking temperature is more suitable for 180-220℃. After cooling, the required craft can be obtained.
[0020] The production line must not stop running during the above process.
[0021] Comparative Example 1 Use a grinding wheel grinder to sand the outer surface of the craft to improve the surface flatness, then use a high-pressure hair dryer to blow away the dust on the outer surface of the craft, then use acetone or anhydrous ethanol solution to rinse the outer surface of the craft, and dry it. Apply the conductive liquid evenly on the outer surface of the craft, and then put it in the oven for preheating. The preheating temperature of the oven is 80℃, and the preheating time is 15min. Use an electrostatic spraying device to evenly spray the powder on the outer surface of the craft. During the spraying process, the thickness of the powder layer should be controlled. It is more appropriate to control the thickness of the powder layer at 60-80um. Spraying is performed intermittently at intervals during the spraying process. Put the craft sprayed with powder into the oven for baking. The baking process needs to go through three stages: heating, heat preservation, and cooling. The baking temperature and time of the oven should be controlled. The baking time is more appropriate for 18-22min and the baking temperature is more appropriate for 180-220℃. After cooling, the required craft can be obtained.
[0022] Comparative Example 2 Use a grinding wheel grinder to sand the outer surface of the craft to improve the surface flatness, then use a high-pressure hair dryer to blow away the dust on the outer surface of the craft, then use acetone or anhydrous ethanol solution to rinse the outer surface of the craft, and dry it. The outer surface of the craft is evenly brushed with conductive liquid, and then placed in an oven for preheating. The preheating temperature of the oven is 80℃, and the preheating time is 15min. Use an electrostatic spraying device to evenly spray the powder on the outer surface of the craft. During the spraying process, the thickness of the powder layer should be controlled well. The thickness of the powder layer is preferably controlled at 60-80um. Put the craft sprayed with powder into the oven for baking. The baking process needs to go through three stages of heating, heat preservation, and cooling. During the above three stages, the heating is interrupted from time to time, the temperature is lowered during the heating process, and the temperature is increased during the cooling process. The baking time is more suitable for 18-22min, and the baking temperature is more suitable for 180-220℃. After cooling, the required craft can be obtained.
[0023] Observe the situation of Example, Comparative Example 1 and Comparative Example 2: In the case of a long abnormal stoppage, the adhesion of the coating on the outer surface of the craft will be significantly reduced, and even a large area of the coating will fall off. Therefore, for the production line, it is necessary to improve the management level, reduce the probability of line stoppage, and take effective measures such as manual intervention in abnormal line stoppage to ensure product quality.
[0024] The purpose of surface pretreatment is to remove the oil and natural oxide film on the surface of aluminum profiles, and then obtain a passivation film through chemical oxidation to greatly enhance the adhesion of the powder coating. Passivation is a key process in pretreatment. The quality of the passivation film will directly affect the quality of powder coating. The passivation film must be dense and the crystals must be uniform. During the pretreatment process, degreasing must be done cleanly. If the oil removal is not thorough, the passivation film will be incomplete, the powder layer will not adhere well, and defects such as shrinkage cavities and pinholes will easily appear on the surface. Profile corrosion will start and spread from then on; the profile surface must be dry, and no moisture can enter the spraying process. The drying temperature should not exceed 130°C to prevent the passivation film from losing too much crystal water and becoming loose, which will reduce the adhesion of the coating.
[0025] The key to the quality of the spray profile surface lies in the control of various process parameters during the spraying process, especially the amount of powder output and the uniformity of powder distribution. In order to ensure the coating quality of the profile, the thickness of the powder layer must be controlled during the powder spraying process. If the powder layer is too thin, the bottom will be exposed and particles will be generated on the surface. If the powder layer is too thick, the coating will produce orange peel, pinholes, flow marks, etc., and the mechanical properties of the profile will also decrease.
[0026] The process of powder curing film formation refers to the process of converting the powder layer electrostatically adsorbed on the surface of the workpiece into a coating that meets the quality requirements through curing treatment. The gelation of the coating mainly occurs in the insulation section. In order to obtain better leveling effect and mechanical properties, the melt aggregation process should be completed as quickly as possible, and there is a longer time to complete leveling and curing. Increase the heating rate of the workpiece, ensure the gelation time of the powder layer, and promote the complete film formation reaction to improve product quality and production efficiency. If the baking time is not enough and the temperature is low, the cross-linking reaction of the coating will be incomplete, affecting the physical and mechanical properties of the coating; conversely, if the baking time is too long and the temperature is too high, it is easy to cause the coating to turn yellow.
[0027] For chemical material manufacturers, due to the differences in surface element composition, chemical reactivity, surface state, etc. between ferrous metals and nonferrous metals, effective regulation of the conversion film deposition rate on various metal surfaces can fundamentally control the film weight and ensure the quality of the coating products. There are many factors that affect adhesion, such as material, water quality, control parameters, treatment effect, powder coating performance, coating thickness, moisture drying and curing effect, working environment, etc. When problems arise, it is necessary to conduct a specific analysis from five aspects: people, machines, materials, methods, and environment to find the cause and find an effective solution.
[0028] The above description is only by way of illustration of certain exemplary embodiments of the present invention. It is undoubted that, for those skilled in the art, the described embodiments can be modified in various ways without departing from the spirit and scope of the present invention. Therefore, the above description is illustrative in nature and should not be construed as limiting the scope of protection of the claims of the present invention.
Claims
1. A high-adhesion electrostatic powder spraying process for iron crafts. Features: The steps include: Step 1: Surface treatment: Use a grinding wheel grinder to sand the outer surface of the craft to improve the surface flatness, then use a high-pressure blower to blow away the dust on the outer surface of the craft, then use a cleaning agent to rinse the outer surface of the craft and dry it in the sun; Step 2: Pretreatment: Evenly apply conductive liquid on the outer surface of the craft, and then put it into the oven for preheating; Step 3: Spraying: Use an electrostatic spraying device to evenly spray the powder onto the outer surface of the craft; Step 4: Powder curing treatment: Put the handicraft sprayed with powder into an oven for baking. The baking process needs to go through three stages: heating, heat preservation, and cooling. After cooling, the desired handicraft can be obtained.
2. According to claim 1, a high-adhesion electrostatic powder spraying process for iron crafts, Features: The cleaning agent in step 1 is acetone or anhydrous ethanol solution.
3. According to claim 1, a high-adhesion electrostatic powder spraying process for iron crafts, Features: The preheating temperature of the oven in step 2 is 80° C. and the preheating time is 15 min.
4. The high-adhesion electrostatic powder spraying process for iron crafts according to claim 1, Features: The pretreatment in step 2 may also be to mix the conductive liquid and ethanol in a certain proportion, evenly apply the mixture on the outer surface of the handicraft, and then air-dry the mixture.
5. According to claim 4, a high-adhesion electrostatic powder spraying process for iron crafts, Features: The ratio of the conductive liquid to ethanol is 1:
50.
6. The high-adhesion electrostatic powder spraying process for iron crafts according to claim 1, Features: During the spraying process described in step 3, the thickness of the powder layer must be controlled well, and it is more appropriate to control the thickness of the powder layer to 60-80um.
7. The high-adhesion electrostatic powder spraying process for iron crafts according to claim 1, Features: In step 4, the baking temperature and time of the oven should be well controlled. The baking time is preferably 18-22 minutes, and the baking temperature is preferably 180-220°C.