Brazing production process and device for single-layer roll-welded pipe and double-layer roll-welded pipe

By adopting brazing process in the production of rolled welded pipes, including the treatment of metal composite sheet strips and electromagnetic induction continuous brazing, the problems of degradation of weld performance and low efficiency in traditional processes are solved, and efficient and stable rolled welded pipe production is achieved , meets the demands of high-end markets and promotes automated production.

CN118976955APending Publication Date: 2024-11-19OKUMTEC TECH WENZHOU CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411158027.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The traditional roll welded pipe production process has problems such as degraded weld performance, low production efficiency, and difficulty in operation automation, which cannot meet the demand of the high-end market.

Method used

The brazing production process of single-layer coil welded pipes and double-layer coil welded pipes, including longitudinal shearing strips and oblique rolling treatment of metal composite plate strips, continuous forming rolling machine sets to form composite pipe blanks, contact resistance preheating and Electromagnetic induction continuous brazing, rapid cooling and quality inspection, combined with automated production lines.

Benefits of technology

It improves the accuracy and stability of the brazing process, improves the performance and production efficiency of rolled welded pipes, reduces costs, meets high-end market demands, and realizes automated production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976955A_ABST
    Figure CN118976955A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of roll-welded pipe machining, in particular to a brazing production process and device for a single-layer roll-welded pipe and a double-layer roll-welded pipe. Comprising the following steps: preparing a metal composite plate strip; longitudinal shearing and splitting are conducted, and the two side parts are subjected to oblique rolling treatment; a continuous forming rolling unit forms a composite pipe blank; carrying out cold rolling on the integrally compounded roll-welded pipe; preheating the contact resistor; electromagnetic induction continuous brazing is conducted; quickly cooling the welded pipe; and brazing quality detection. According to the brazing production process and device for the single-layer roll-welded pipe and the double-layer roll-welded pipe, the production efficiency is improved, the production cost is reduced, the performance of roll-welded pipe products is remarkably improved, and the requirements of the market for high-end roll-welded pipe products are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coiled welded pipe processing, and in particular to a brazing production process and device for a single-layer coiled welded pipe and a double-layer coiled welded pipe. Background Art

[0002] In modern industrial production, coiled welded pipes have become indispensable materials due to their excellent performance and wide range of applications. The production technology of coiled welded pipes has undergone a transformation from traditional welding technology to modern brazing technology. Compared with traditional welding technology, brazing technology has the advantages of high weld strength, uniform weld, and high production efficiency. However, with the continuous advancement of industrial technology, the performance requirements for coiled welded pipes are getting higher and higher, and traditional brazing technology can no longer fully meet market demand. Therefore, it is particularly important to develop a new brazing production process and device for single-layer coiled welded pipes and double-layer coiled welded pipes.

[0003] The traditional production method of coiled welded pipe mainly adopts arc welding, laser welding and other welding technologies. These technologies are easy to produce heat-affected zones during the welding process, resulting in the degradation of material properties in the weld area, such as reduced hardness and weakened corrosion resistance. In addition, the production efficiency of traditional welding methods is low, and the technical requirements for operators are high, making it difficult to achieve automated production. Therefore, in order to improve the quality and production efficiency of coiled welded pipes and reduce production costs, the development of a new brazing production process and device has become an inevitable trend in the development of the industry.

[0004] In the prior art, although there are some brazing processes, these processes often have some limitations, such as inaccurate brazing temperature control, uneven brazing speed, unstable brazing quality, etc. The existence of these problems limits the application of coiled welded pipes in high-end fields.

[0005] Therefore, the present invention proposes a novel brazing production process and device for single-layer rolled welded pipe and double-layer rolled welded pipe, aiming to solve the problems existing in the prior art, improve the accuracy and stability of the brazing process, and thus produce rolled welded pipe products with better performance. Summary of the invention

[0006] The present invention provides a brazing production process and device for single-layer rolled welded pipes and double-layer rolled welded pipes, which not only improves production efficiency and reduces production costs, but also significantly improves the performance of rolled welded pipe products and meets the market demand for high-end rolled welded pipe products.

[0007] The technical solution adopted by the present invention is: a brazing production process for a single-layer rolled welded pipe and a double-layer rolled welded pipe, comprising the following steps:

[0008] Step 1: Prepare metal composite plate strip: select metal composite plate strip with a total thickness of 0.1-1.5 mm;

[0009] Step 2, longitudinal shearing and striping and oblique rolling of both sides: longitudinally shearing the metal composite plate strip into strips, and obliquely rolling the two sides of the metal composite plate strip through an edge bevel rolling mill to form a wedge-shaped overlapping bevel with a certain angle;

[0010] Step 3, forming a composite tube blank by a continuous forming rolling unit: continuously cold-bending the metal composite plate strip into a composite tube blank by a continuous forming rolling unit;

[0011] Step 4, cold rolling the composite tube into an integrated coiled welded tube: the overlapping inclined surface of the composite tube blank is cold rolled in the roller pass using a roller and a mandrel to form an integrated thin-walled coiled welded tube with equal wall thickness in the circumferential direction;

[0012] Step 5: Contact resistance preheating: Place the coiled welded pipe into the contact resistance preheating device for rapid and uniform heating;

[0013] Step 6, electromagnetic induction continuous brazing: the preheated coiled welded pipe is placed into the induction heating coil of the electromagnetic induction continuous brazing device, and the coiled welded pipe is continuously brazed by duplex heating in a protective gas;

[0014] Step 7, rapid cooling of the welded pipe: After continuous brazing, the coiled welded pipe enters the pipe rapid cooling device to rapidly cool the coiled welded pipe;

[0015] Step 8, brazing quality inspection: The brazing temperature, brazing speed, brazing quality, pipe diameter tolerance, roundness tolerance and surface quality are inspected and feedback is given through the pipe body brazing quality inspection device.

[0016] As a further improvement of the present invention, the metal composite plate strip is composed of a base metal and cladding metals located on both sides of the base metal, wherein the cladding metals account for 3%-20% of the total thickness of the metal composite plate strip.

[0017] As a further improvement of the present invention, the base metal is made of high-strength and high-melting-point metal, including steel, stainless steel, and titanium; the cladding metal is made of low-melting-point metal, specifically copper, and the cladding metal and the base metal are composited into one through rolling composite, casting and rolling composite, and reverse solidification process.

[0018] As a further improvement of the present invention, the edge bevel treatment is achieved by oblique rolling, which can be pre-processed offline or online; the bevels are overlapped after the tube blank is circumferentially formed, and the overlap width is 0.5-3 times the strip thickness.

[0019] As a further improvement of the present invention, the pipe rapid cooling device adopts low-temperature circulating water cooling, low-temperature gas blowing slow cooling, liquefied nitrogen, and liquefied carbon dioxide ultra-low temperature gas rapid cooling technology.

[0020] As a further improvement of the present invention, the temperature of the resistance preheating device is controlled at 700-900°C; the current frequency of the electromagnetic induction continuous brazing device is 10-100KHz, and the temperature of the electromagnetic induction continuous brazing device is controlled at ≤1200°C; the conveying speed of the coiled welded pipe is 20-80m / min.

[0021] As a further improvement of the present invention, the protective gas is an inert gas, including one of nitrogen, argon, helium, and a nitrogen-hydrogen mixed gas.

[0022] A brazing production device for single-layer coiled welded pipe and double-layer coiled welded pipe, including a strip uncoiler, a steering roller and an edge bevel rolling mill, a continuous forming rolling unit, a resistance preheating device, an electromagnetic induction continuous brazing device, an exhaust gas collection and purification device, a pipe rapid cooling device, a pipe body brazing quality detection device, a surface passivation and drying device, a traction roller, a cutter, a discharging steering roller, and a coiler, which are sequentially connected to form a complete production line.

[0023] As a further improvement of the present invention, the resistance preheating device is composed of a resistance heating conductive voltage head, a resistance heating conductive support wheel, and a resistance heating conductive voltage wheel, and the resistance heating conductive support wheel and the resistance heating conductive voltage wheel are respectively located below and above the coiled welded pipe;

[0024] The induction heating coil of the electromagnetic induction continuous brazing device is made of 4-12m hollow pure copper rectangular tube and round tube. Water is passed through the copper tube for cooling during operation. The thickness of the copper tube wall is less than the current penetration depth, specifically 1-3mm. At the same time, the size and number of turns of the induction heating coil are designed according to the specifications, material characteristics, mechanical properties, surface requirements and brazing efficiency of the coiled welded pipe to ensure the best heating effect and production efficiency.

[0025] As a further improvement of the present invention, the induction heating coil is fixed by clamping and positioning the workpiece, and there is a gap between the induction heating coil and the coiled welded pipe, specifically 0.38-0.5 mm.

[0026] Beneficial effects of the present invention:

[0027] (1) By precisely controlling the brazing temperature and speed, the brazing quality of the coiled pipe is significantly improved, weld defects are reduced, and the overall performance and reliability of the product are improved.

[0028] (2) The continuous forming rolling unit and cold rolling composite process adopted have greatly improved production efficiency, shortened production cycle, and reduced energy consumption and material loss.

[0029] (3) Through the combination of contact resistance preheating and electromagnetic induction continuous brazing technology, rapid and uniform heating is achieved, effectively avoiding the formation of heat-affected zone and ensuring the material properties of the weld area.

[0030] (4) The present invention uses a rapid cooling device for pipe fittings, so that the rolled welded pipe can be quickly cooled in a short time, reducing thermal deformation and residual stress, and improving the dimensional accuracy and roundness tolerance of the product.

[0031] (5) The present invention ensures that the brazing quality of each roll of welded pipe meets the standard through the design of the brazing quality detection device, thus providing a reliable guarantee for product quality.

[0032] (6) The production device of the present invention has a compact structure and a high degree of automation, which reduces the technical requirements for operators, reduces labor intensity, and facilitates large-scale production.

[0033] (7) The shielding gas used in the present invention ensures safety and environmental protection during the welding process, avoids the generation of harmful gases, and protects the health of operators and the cleanliness of the environment.

[0034] (8) The production process and device of the present invention are suitable for the production of single-layer and double-layer rolled welded pipes of different specifications and materials, and have broad market application prospects and economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 It is a schematic diagram of the production line structure of a brazing production process and device for a single-layer coiled welded pipe and a double-layer coiled welded pipe of the present invention;

[0036] Figure 2 It is a schematic diagram of the structure of a resistance preheating device and an electromagnetic induction continuous brazing device of a brazing production process and device of a single-layer coiled welded pipe and a double-layer coiled welded pipe of the present invention;

[0037] Figure 3 It is a schematic diagram of the metal composite plate strip structure of a brazing production process and device for a single-layer rolled welded pipe and a double-layer rolled welded pipe of the present invention;

[0038] Figure 4 It is a schematic diagram of the process of processing a metal composite plate strip into a coiled material in a brazing production process and device of a single-layer coiled welded pipe and a double-layer coiled welded pipe of the present invention;

[0039] Figure 5 The invention discloses a process flow chart of the brazing production process and device of a single-layer rolled welded pipe and a double-layer rolled welded pipe.

[0040] As shown in the figure: 1. Strip uncoiler; 2. Metal composite plate strip; 2.1. Base metal; 2.2. Cladding metal; 3. Turning roller and edge bevel rolling mill; 4. Continuous forming rolling unit; 5. Resistance preheating device; 5.1. Resistance heating conductive voltage head; 5.2. Resistance heating conductive support wheel; 5.3. Resistance heating conductive voltage wheel; 6. Electromagnetic induction continuous brazing device; 6.1. Induction heating coil; 6.2. Clamping and positioning workpiece; 7. Waste gas collection and purification device; 8. Pipe fitting rapid cooling device; 9. Pipe body brazing quality detection device; 10. Surface passivation and drying device; 11. Pulling roller; 12. Cutter; 13. Discharging turning roller; 14. Coiler. DETAILED DESCRIPTION

[0041] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0042] The present invention provides the following Figure 1-5 The brazing production process of a single-layer rolled welded pipe and a double-layer rolled welded pipe shown includes the following steps:

[0043] Step 1, preparing a metal composite plate strip: selecting a metal composite plate strip 2 with a total thickness of 0.3-1.5 mm;

[0044] Step 2, longitudinal shearing and striping and oblique rolling of both sides: longitudinally shearing the metal composite plate strip 2 into strips, and obliquely rolling the two sides of the metal composite plate strip 2 through an edge bevel rolling mill to form a wedge-shaped overlapping bevel with a certain angle;

[0045] Step 3, forming a composite tube blank by a continuous forming rolling unit: continuously cold-bending the metal composite plate strip 2 into a composite tube blank by a continuous forming rolling unit 4;

[0046] Step 4, cold rolling the composite tube into an integrated coiled welded tube: the overlapping inclined surface of the composite tube blank is cold rolled in the roller pass using a roller and a mandrel to form an integrated thin-walled coiled welded tube with equal wall thickness in the circumferential direction;

[0047] Step 5, contact resistance preheating: the coiled welded pipe is placed in the contact resistance preheating device 5 for rapid and uniform heating;

[0048] Step 6, electromagnetic induction continuous brazing: the preheated coiled welded pipe is placed into the induction heating coil 6.1 of the electromagnetic induction continuous brazing device 6, and the coiled welded pipe is continuously brazed by duplex heating in a protective gas;

[0049] Step 7, rapid cooling of the welded pipe: After continuous brazing, the coiled welded pipe enters the pipe rapid cooling device 8 to rapidly cool the coiled welded pipe;

[0050] Step eight, brazing quality inspection: the brazing temperature, brazing speed, brazing quality, pipe diameter tolerance, roundness tolerance and surface quality are inspected and fed back by the pipe body brazing quality inspection device 9 .

[0051] In the present invention, the metal composite plate strip 2 is composed of a base metal 2.1 and cladding metals 2.2 located on both sides of the base metal, wherein the cladding metals 2.2 account for 3%-20% of the total thickness of the metal composite plate strip 2.

[0052] In the present invention, the base metal 2.1 is made of high-strength and high-melting-point metal, including steel, stainless steel, and titanium; the cladding metal 2.2 is made of low-melting-point metal, specifically copper, and the cladding metal 2.2 and the base metal 2.1 are combined into one by rolling composite, casting and rolling composite, and reverse solidification process.

[0053] The edge bevel treatment in the present invention is achieved by oblique rolling, which can be pre-processed offline or online; the bevels are overlapped after the tube blank is circumferentially formed, and the overlap width is 0.5-3 times the strip thickness.

[0054] The pipe rapid cooling device 8 of the present invention adopts low-temperature circulating water cooling, low-temperature gas blowing slow cooling, liquefied nitrogen or liquefied carbon dioxide ultra-low temperature gas rapid cooling technology.

[0055] In the present invention, the temperature of the resistance preheating device 5 is controlled at 700-900°C; the current frequency of the electromagnetic induction continuous brazing device 6 is 10-100KHz, and the temperature of the electromagnetic induction continuous brazing device 6 is controlled at ≤1200°C; the conveying speed of the coiled welded pipe is 20-80m / min.

[0056] The protective gas in the present invention is an inert gas, including one of nitrogen, argon, helium, and nitrogen-hydrogen mixed gas.

[0057] A brazing production device for single-layer coiled welded pipe and double-layer coiled welded pipe, characterized in that it includes a strip uncoiler 1, a steering roller and edge bevel rolling mill 3, a continuous forming rolling unit 4, a resistance preheating device 5, an electromagnetic induction continuous brazing device 6, an exhaust gas collection and purification device 7, a pipe rapid cooling device 8, a pipe body brazing quality detection device 9, a surface passivation and drying device 10, a traction roller 11, a cutter 12, a discharge steering roller 13, and a coiler 14, which are sequentially connected to form a complete production line.

[0058] In the present invention, the resistance preheating device 5 is composed of a resistance heating conductive voltage head 5.1, a resistance heating conductive support wheel 5.2, and a resistance heating conductive voltage wheel 5.3, and the resistance heating conductive support wheel 5.2 and the resistance heating conductive voltage wheel 5.3 are respectively located below and above the coiled welded pipe; the induction heating coil 6.1 of the electromagnetic induction continuous brazing device 6 is made of a 4-12m hollow pure copper rectangular tube or round tube, and water is passed through the copper tube for cooling during operation. The thickness of the copper tube wall is less than the current penetration depth, specifically 1-3mm. At the same time, the size and number of turns of the induction heating coil 6.1 are designed according to the specifications, material characteristics, mechanical properties, surface requirements, and brazing efficiency of the coiled welded pipe to ensure the best heating effect and production efficiency.

[0059] In the present invention, the induction heating coil 6.1 is fixed by clamping and positioning the workpiece 6.2, and there is a gap between the induction heating coil 6.1 and the coiled welded pipe, specifically 0.38-0.5 mm.

[0060] Example:

[0061] In order to further illustrate the implementation of the brazing production process and device of a single-layer rolled welded pipe and a double-layer rolled welded pipe of the present invention, a specific production example is provided below:

[0062] In this embodiment, a metal composite plate strip 2 with a thickness of 0.8 mm is selected, wherein the base metal 2.1 is stainless steel and the cladding metal 2.2 is copper.

[0063] (i) First, the metal composite plate strip 2 is uncoiled by the strip uncoiler 1, and then slitting is performed to form a desired width. Then, the edge of the metal composite plate strip 2 is obliquely rolled by the steering roller and the edge bevel rolling mill 3 to form a wedge-shaped overlapping bevel.

[0064] (ii) Subsequently, the processed metal composite plate strip 2 is fed into a continuous forming rolling unit 4, and the metal composite plate strip 2 is rolled into a desired composite tube blank through the cooperation of a series of rolling rollers and a mandrel.

[0065] (III) Next, the composite tube blank is sent to the contact resistance preheating device 5 for preheating. In this embodiment, the temperature of the resistance preheating device 5 is controlled at 700° C.-800° C. to ensure that the coil reaches an appropriate temperature before entering the electromagnetic induction continuous brazing device 6.

[0066] (IV) In the electromagnetic induction continuous brazing device 6, the coil is continuously brazed by double heating through the induction heating coil 6.1 in an environment of protective gas (argon in this example). In this embodiment, the current frequency of the induction heating coil 6.1 is set to 50KHz and the temperature is controlled at 1100°C to ensure the brazing effect.

[0067] (V) After continuous brazing, the coiled welded pipe enters the pipe fast cooling device 8 for fast cooling. In this embodiment, an ultra-low temperature circulating water cooling (10°C-15°C) process is adopted to ensure fast cooling of the coiled welded pipe and prevent degradation of material properties due to overheating.

[0068] (VI) Finally, the brazing temperature, brazing speed, brazing quality, pipe diameter tolerance, roundness tolerance and surface quality are tested and fed back by the pipe body brazing quality detection device 9. In this embodiment, all the detection indicators meet the predetermined technical requirements, ensuring the quality of the coiled welded pipe.

[0069] Through the above steps, this embodiment successfully produces single-layer rolled welded pipes and double-layer rolled welded pipes that meet the technical requirements. The implementation of the present invention not only improves production efficiency, but also ensures product quality and has good application prospects.

[0070] In summary, the brazing production process and device of the single-layer rolled welded pipe and double-layer rolled welded pipe of the present invention, which is efficient, stable, energy-saving and environmentally friendly, has broad application prospects and market competitiveness. Through the implementation of the present invention, the market demand for high-quality rolled welded pipes can be met, and the development of related industries can be promoted.

[0071] The above implementation modes are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned implementation modes, a person skilled in the art should understand that the technical solutions described in the aforementioned implementation modes can still be modified, or some of the technical features can be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the implementation modes of the present invention.

Claims

1. A brazing production process for single-layer coiled welded pipe and double-layer coiled welded pipe, characterized in that: The following steps are involved: Step 1, preparing a metal composite plate strip: selecting a metal composite plate strip (2) with a total thickness of 0.1-1.5 mm; Step 2, longitudinal shearing and stripping, and oblique rolling treatment of both sides: longitudinally shearing the metal composite plate strip (2) into strips, and obliquely rolling the two sides of the metal composite plate strip (2) through an edge bevel rolling mill to form a wedge-shaped overlapping bevel with a certain angle; Step 3, forming a composite tube blank by a continuous forming rolling unit: continuously cold-bending the metal composite plate strip (2) into a composite tube blank by a continuous forming rolling unit (4); Step 4, cold rolling the composite tube into an integrated coiled welded tube: the overlapping inclined surface of the composite tube blank is cold rolled in the roller pass using a roller and a mandrel to form an integrated thin-walled coiled welded tube with equal wall thickness in the circumferential direction; Step 5, contact resistance preheating: placing the coiled welded pipe into a contact resistance preheating device (5) for rapid and uniform heating; Step 6, electromagnetic induction continuous brazing: the preheated coiled welded pipe is placed into the induction heating coil (6.1) of the electromagnetic induction continuous brazing device (6), and continuous duplex heating brazing is performed on the coiled welded pipe in a protective gas; Step 7, rapid cooling of the welded pipe: after continuous brazing, the coiled welded pipe enters a pipe rapid cooling device (8) to rapidly cool the coiled welded pipe; Step 8, brazing quality inspection: the brazing temperature, brazing speed, brazing quality, pipe diameter tolerance, roundness tolerance and surface quality are inspected and fed back by the pipe body brazing quality inspection device (9).

2. The brazing production process of a single-layer rolled welded pipe and a double-layer rolled welded pipe according to claim 1 is characterized in that: The metal composite plate strip (2) is composed of a base metal (2.1) and cladding metals (2.2) located on both sides of the base metal, wherein the cladding metals (2.2) account for 3%-20% of the total thickness of the metal composite plate strip (2).

3. The brazing production process of a single-layer coiled welded pipe and a double-layer coiled welded pipe according to claim 2 is characterized in that: The base metal (2.1) is made of high-strength and high-melting-point metal, including steel, stainless steel, and titanium; the cladding metal (2.2) is made of low-melting-point metal, specifically copper; the cladding metal (2.2) and the base metal (2.1) are combined into one through rolling composite, casting and rolling composite, and reverse solidification processes.

4. The brazing production process of a single-layer coiled welded pipe and a double-layer coiled welded pipe according to claim 1, characterized in that: The edge bevel treatment is achieved by oblique rolling, which can be pre-processed offline or online; the bevels are overlapped after the tube blank is circumferentially formed, and the overlap width is 0.5-3 times the strip thickness.

5. The brazing production process of a single-layer coiled welded pipe and a double-layer coiled welded pipe according to claim 1 is characterized in that: The pipe rapid cooling device (8) adopts low-temperature circulating water cooling, low-temperature gas blowing slow cooling, liquefied nitrogen, and liquefied carbon dioxide ultra-low temperature gas rapid cooling processes.

6. The brazing production process of a single-layer coiled welded pipe and a double-layer coiled welded pipe according to claim 1, characterized in that: The temperature of the resistance preheating device (5) is controlled at 700-900°C; the current frequency of the electromagnetic induction continuous brazing device (6) is 10-100KHz, and the temperature of the electromagnetic induction continuous brazing device (6) is controlled at ≤1200°C; the conveying speed of the coiled welded pipe is 20-80m / min.

7. The brazing production process of a single-layer coiled welded pipe and a double-layer coiled welded pipe according to claim 1, characterized in that: The protective gas is an inert gas, including one of nitrogen, argon, helium, and a nitrogen-hydrogen mixed gas.

8. A brazing production device for single-layer coiled welded pipe and double-layer coiled welded pipe, characterized in that: The invention comprises a strip unwinder (1), a turning roller and an edge bevel rolling mill (3), a continuous forming rolling unit (4), a resistance preheating device (5), an electromagnetic induction continuous brazing device (6), an exhaust gas collecting and purifying device (7), a pipe fitting rapid cooling device (8), a pipe body brazing quality detection device (9), a surface passivation and drying device (10), a traction roller (11), a cutter (12), a discharge turning roller (13), and a coiler (14), which are sequentially connected to form a complete production line.

9. The brazing production device for single-layer coiled welded pipe and double-layer coiled welded pipe according to claim 8, characterized in that: The resistance preheating device (5) is composed of a resistance heating conductive voltage head (5.1), a resistance heating conductive support wheel (5.2), and a resistance heating conductive voltage wheel (5.3), and the resistance heating conductive support wheel (5.2) and the resistance heating conductive voltage wheel (5.3) are respectively located below and above the coiled welded pipe; The induction heating coil (6.1) of the electromagnetic induction continuous brazing device (6) is made of 4-12m hollow pure copper rectangular tubes and round tubes. Water is passed through the copper tube for cooling during operation. The thickness of the copper tube wall is less than the current penetration depth, specifically 1-3mm. At the same time, the size and number of turns of the induction heating coil (6.1) are designed according to the specifications, material characteristics, mechanical properties, surface requirements and brazing efficiency of the coiled welded tube to ensure the best heating effect and production efficiency.

10. The brazing production device for single-layer coiled welded pipe and double-layer coiled welded pipe according to claim 9, characterized in that: The induction heating coil (6.1) is fixed by clamping and positioning the workpiece (6.2), and there is a gap between the induction heating coil (6.1) and the coiled welded pipe, specifically 0.38-0.5 mm.

Citation Information

Cited By

  • Copper-iron composite material roll-welded pipe, welding process and welding device

    CN119658093A

  • Copper-iron composite material coiled welded pipe, welding process and welding device

    CN119658093B