Bentonite for manual welding rod and manual welding rod

By using bentonite with a particle size of less than 58μm in the hand electrode skin and combining with water glass medium, the problem of defects and defects in the high-speed production of hand electrode skin is solved, the coating properties and peel resistance are improved, and high efficiency is achieved Production and low cost welding rod manufacturing.

CN118977015APending Publication Date: 2024-11-19KUSN GINTUNE WELDING
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411237755.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Existing hand electrode skins are prone to defects and defects in high-speed mass production, and customers with high appearance requirements are difficult to meet. In the existing technology, alginate and carboxymethyl cellulose sodium are difficult to ensure at high speeds. The density and anti-stripping properties of the drug skin.

Method used

Use bentonite with a particle size of less than 58μm, with a content of more than 30% of the total mass of the drug skin, and combine it with water glass media to improve the adhesiveness and lubricity of the drug skin, replace alginate and sodium carboxymethylcellulose to enhance the The strength and coating properties of the medicine skin.

Benefits of technology

The coating and peel resistance of hand welding rod skins are significantly improved, the generation rate of poor welding rods is reduced, the production efficiency is improved, and the cost is reduced, and the yield rate reaches more than 99.5%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005028242940000041
    Figure BDA0005028242940000041
  • Figure BDA0005028242940000051
    Figure BDA0005028242940000051
  • Figure BDA0005028242940000052
    Figure BDA0005028242940000052
Patent Text Reader

Abstract

The invention discloses bentonite for a manual welding rod and the manual welding rod, and according to the mass ratio, the content of particles with the particle size smaller than 58 microns in the bentonite for the manual welding rod accounts for 30% or above of all particles. The coating of the manual welding rod contains bentonite which accounts for 0.2-1.6% of the total mass of the coating and is used for the manual welding rod. The welding rod is manufactured by adding the special bentonite, so that the coating of the welding rod is very excellent in production coating performance and stripping resistance, the occurrence of poor manufacturing conditions in the conventional manual welding rod production process is reduced, and the welding rod is particularly suitable for large-batch production and manufacturing of manual welding rods.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of welding materials, and in particular to bentonite for hand welding rods and hand welding rods which have good coating properties and can suppress adverse conditions from occurring during the manufacture of hand welding rods. Background Art

[0002] It is well known that adding alginate and sodium carboxymethyl cellulose to the coating of hand welding rods can improve the coating's ...

[0003] However, even if the above technology is used to produce hand welding rods, the tightness of the coating after coating around the core wire will be insufficient. When large-scale coating is carried out at a higher speed, the newly coated welding rod will not be able to withstand the impact force generated by the collision with the brake, and this collision will cause more obvious flaws and defects on the surface of the finished hand welding rod coating.

[0004] In addition, various customers in the equipment manufacturing industries, whether petrochemical, boiler, or nuclear power, have increasingly higher requirements for the appearance of hand welding rods, so it is necessary to develop a coating with better paintability than in the past. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a bentonite for hand welding rods and a hand welding rod prepared therefrom. The bentonite has good adhesion, plasticity and good lubrication performance in water and water glass media, thereby improving the strength of the welding rod coating, reducing the heat generation of powder and improving the cracking of the welding rod coating, and significantly improving the paintability of the welding rod coating. The addition of the bentonite not only improves the production efficiency of the welding rod, but also can suppress the occurrence of manufacturing defects during high-speed and large-scale production of welding rods.

[0006] The technical solution of the present invention is a bentonite for hand welding rods, wherein the content of particles with a particle size of less than 58 μm in the bentonite for hand welding rods accounts for more than 30% of all particles in terms of mass ratio.

[0007] The bentonite for hand welding rods can be applied to the preparation of the coatings of titanium type, calcium titanium type, ilmenite type and low hydrogen type welding rods.

[0008] The present invention also provides a hand welding rod, which has a core wire made of carbon steel or alloy steel and is coated with a coating around the core wire; the coating contains 0.2-1.6% of the bentonite for the hand welding rod by weight.

[0009] The hand welding rod of the present invention uses bentonite to replace alginate and sodium carboxymethyl cellulose that must be added to the conventional welding rod coating, effectively reducing the cost of the welding rod coating. When the content of the bentonite particles with a particle size of less than 58 μm is more than 30 mass % (hereinafter referred to as %), the yield rate of the welding rod in high-speed mass production can reach more than 99.5%.

[0010] The inventors have conducted various studies to develop a method for improving the coating coating properties. First, in order to improve the swelling properties of bentonite for hand welding rods and water glass, bentonite for hand welding rods was added to water glass and mixed, and this mixture was mixed with the raw materials of the coating and applied to the core wire to evaluate the coating coating properties. However, even with this method, the tightness of the coating became uneven, and good coating properties could not be obtained.

[0011] Then, the content of bentonite for welding rods in the coating was changed and the coating's paintability was evaluated. However, even if the content of bentonite for hand welding rods in the coating was increased, although the occurrence of defective welding rods after coating could be reduced and the paintability could be improved, the coating's anti-peeling and moisture absorption properties would be reduced, and satisfactory results could not be obtained.

[0012] Therefore, the inventors have conducted repeated and in-depth research and found that by adjusting the particle size of bentonite for hand welding rods, the coating property of the coating can be improved, thereby improving the production efficiency of welding rods. In other words, in order to make the coating property of the coating good, it is very effective to use bentonite for hand welding rods with a smaller particle size.

[0013] The following is an explanation of the reasons for limiting the particle size of bentonite used in hand welding rods and its content in the coating.

[0014] If the content of bentonite for hand welding rods with a particle size of less than 58μm is less than 30% relative to the total mass, the coating property and the peeling resistance of the coating will be reduced. On the other hand, if the content of bentonite for hand welding rods with a particle size of less than 58μm is more than 30% relative to the total mass, when the bentonite is contained in the coating, the bentonite will swell evenly in the coating and improve the water retention. As a result, the compactness of the coating is improved, which can prevent the occurrence of flaws and defects in the coating after coating, and can also significantly improve the peeling resistance of the coating. Therefore, in the bentonite for hand welding rods, the content of particles with a particle size of less than 58μm should be controlled to be more than 30%.

[0015] If the content of the bentonite for hand welding rods having a specified particle size in the coating is less than 0.2% relative to the total mass of the coating, even if the bentonite for hand welding rods is used, the effect of improving the coating properties cannot be obtained. In addition, the compactness of the coating will deteriorate and the peeling resistance will decrease. On the other hand, if the content of the bentonite for hand welding rods in the coating exceeds 1.6%, although the coating properties will become excellent, the peeling resistance will decrease. Therefore, the content of the bentonite for hand welding rods in the coating should be controlled at 0.2-1.6% relative to the total mass of the coating.

[0016] In addition, the bentonite for hand welding rods of the present invention can be applied to the coating of titanium type, calcium titanium type, ilmenite type and low hydrogen type welding rods.

[0017] Next, the bentonite for hand welding rod and the hand welding rod of the present invention are compared with the embodiments and comparative examples and described in detail.

[0018] First, the bentonite for hand welding rods with a particle size distribution as shown in Table 1 below was prepared, and then the bentonite was mixed with carbonate, silicate, fluoride, organic matter, alloying agent and other powders according to a certain formula ratio and stirred evenly, and a certain amount of mixed water glass was added, and wet mixed for a period of time to form a sticky mud electrode coating. After setting the coating to contain 0.8% bentonite relative to the total mass of the coating, the coating was actually applied on the core wire to evaluate the coating's coating and anti-stripping properties. These evaluation results are summarized in Table 1.

[0019] In the evaluation results and comprehensive evaluation columns of the coating peeling resistance shown in Table 1 below, ◎ indicates excellent evaluation results, ○ indicates good, □ indicates poor, and △ indicates very poor. In addition, in the column of defective electrode generation rate after coating, 0 to 10 (kg / ton) is evaluated as ◎, 11 to 50 (kg / ton) is evaluated as ○, 51 to 100 (kg / ton) is evaluated as □, and 101 (kg / ton) and above is evaluated as △.

[0020] Table 1

[0021]

[0022] As shown in Table 1, in Examples A, B, and C, since the content of particles with a particle size of 58 μm or less in the bentonite is more than 30%, the evaluation results of the coating properties are good, and the yield rate is as high as more than 99.5%. On the other hand, in Comparative Examples D and E, since the content of particles with a particle size of 58 μm or less in the bentonite is less than 30%, the rate of defective electrodes after coating increases, and good results cannot be obtained for the peeling resistance of the coating.

[0023] Next, the bentonite shown in Table 1 above was added in different amounts to the formulas of the four types of coatings shown in Table 2 below, namely, titanium type (E4313), calcium titanium type (E4303), ilmenite type (E4319), and low hydrogen type (E4315), and the coatings were prepared by mixing them. Then, the coating properties of the coatings were evaluated by actually coating the core wires, that is, the amount of defective electrodes caused by flaws and defects in the coatings on the coated electrodes and the peeling resistance were evaluated.

[0024] The manufacturing conditions and evaluation results of titanium type welding rods are shown in Table 3 below, the manufacturing conditions and evaluation results of titanium calcium type welding rods are shown in Table 4 below, the manufacturing conditions and evaluation results of ilmenite type welding rods are shown in Table 5 below, and the manufacturing conditions and evaluation results of low hydrogen type welding rods are shown in Table 6 below.

[0025] Table 2 Flux composition of different types of welding rods

[0026]

[0027] Table 3 Manufacturing conditions and evaluation results of titanium welding rods

[0028]

[0029]

[0030] Table 4 Manufacturing conditions and evaluation results of titanium calcium type welding rods

[0031]

[0032] Table 5 Manufacturing conditions and evaluation results of ilmenite type welding rods

[0033]

[0034]

[0035] Table 6 Manufacturing conditions and evaluation results of low hydrogen welding rods

[0036]

[0037] As shown in Tables 3 to 6, in Examples 1 to 3, 9 to 11, 17 to 19 and 25 to 27, since the particle size of the bentonite and its content in the coating are within the range specified in the present invention, the coating property of the welding rod is relatively good, thereby reducing the amount of defective products produced after coating. At the same time, the welding rod also has excellent anti-peeling properties, which can improve production efficiency.

[0038] On the other hand, in Comparative Examples 4, 12, 20 and 28, since the content of bentonite in the coating exceeded the upper limit value specified in the present invention, although the amount of defective products after coating was small, the peeling resistance was poor. In Comparative Examples 5, 6, 13, 14, 21, 22, 29 and 30, since no bentonite was added or the amount added did not meet the lower limit value of the present invention, the amount of defective products after coating was high and the peeling resistance was also poor in the production of ilmenite type and low hydrogen type welding rods.

[0039] In addition, in Comparative Examples 7, 15, 23 and 31, although the content of bentonite used in the coating is within the range specified in the present invention, the particle size distribution of the bentonite is outside the range specified in the present invention, resulting in a high amount of defective products after coating and low production efficiency. In Comparative Examples 8, 16, 24 and 32, although the content of bentonite used in the coating is within the range of the present invention, the content added is less than that of Comparative Examples 7, 15, 23 and 31, and the particle size distribution of the bentonite is not within the range of the present invention, resulting in a large amount of defective products after coating and low production efficiency.

[0040] It can be seen from the above that the present invention can achieve the same excellent effect in any type of hand welding rod, such as titanium type, calcium titanium type, ilmenite type and low hydrogen type.

[0041] The present invention stipulates the particle size of the bentonite for hand welding rods and limits the content of the bentonite for hand welding rods in the welding rod coating. When the coating added with the bentonite for hand welding rods is applied to the core wire, the coating property of the welding rod can be significantly improved, thereby improving the production efficiency of hand welding rods and reducing the occurrence of manufacturing defects.

[0042] The above is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several modifications and improvements without departing from the inventive concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. A bentonite for hand welding rod, characterized in that: In terms of mass ratio, the content of particles of the bentonite for hand welding electrodes having a particle size of less than 58 μm accounts for more than 30% of all particles.

2. The use of bentonite for hand welding rods as claimed in claim 1, characterized in that: The bentonite for hand welding rods is applied to the preparation of the coatings of titanium type, calcium titanium type, ilmenite type and low hydrogen type welding rods.

3. A hand welding rod, characterized in that: The hand welding rod has a core wire made of carbon steel or alloy steel, and a coating is applied around the core wire; the coating contains the bentonite for hand welding rod according to claim 1, which accounts for 0.2 to 1.6% of the total mass of the coating.