Preparation method of ultra-high molecular weight polyethylene nanofiber composite membrane

Through island spinning and crystal structure regulation, combined with liquid paraffin preswelling and the use of nucleating agents, the preparation of ultra-high molecular weight polyethylene nanofibers was achieved, and the problem of uneven pore size of UHMWPE battery separator was solved, and excellent lyophilic was obtained and tensile strength, suitable for battery separator materials.

CN118977360APending Publication Date: 2024-11-19WUHAN TEXTILE UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410956883.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The preparation of ultra-high molecular weight polyethylene (UHMWPE) nanofibers has problems such as poor melt flowability and difficult molding processing. Especially, nanofibers with a size below 300 nm are difficult to prepare. The existing technology is costly and low in efficiency, and commercialization is facing costs. , process and quality control challenges.

Method used

Using a combination of island spinning and crystal structure regulation, the two-component extrusion, stretching and grain refinement are used to perform online crystal regulation using liquid paraffin preswelling and nucleating agent, combined with acetone extraction and wet coating Covering technology realizes batch preparation of UHMWPE nanofibers and composite membrane production with adjustable pore size.

Benefits of technology

UHMWPE nanofibers with a diameter of less than 300nm were successfully prepared, which has excellent lyophilicity and tensile strength, which solved the problem of uneven pore size and difficulty in preparing the UHMWPE battery separator and met the performance requirements of battery separator materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118977360A_ABST
    Figure CN118977360A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method of an ultra-high molecular weight polyethylene nanofiber composite membrane. The method comprises the following steps: firstly, carrying out liquid paraffin pre-swelling on UHMWPE powder (the ratio of UHMWPE to liquid paraffin is 2: 8), then carrying out melt blending on the swelled UHMWPE gel, a nucleating agent and CAB by using a twin-screw extruder, drafting and refining the UHMWPE by virtue of UHMWPE online crystal regulation and control in an extrusion process and stretching and extruding effects of CAB blending on the UHMWPE, then extracting a CAB phase and liquid paraffin by adopting acetone, and finally, carrying out melt blending on the CAB and the UHMWPE by using a twin-screw extruder. UHMWPE nanofibers with the particle size being smaller than 300 nm are obtained, and then the ultra-high molecular weight polyethylene nanofiber composite membrane with the adjustable pore diameter and thickness is obtained through a layer-by-layer wet coating technology. According to the method, the UHMWPE nanofibers with the particle size being smaller than 300 nm are obtained through the method of combining sea-island spinning and crystal structure regulation and control, the obtained composite membrane can be used for a battery diaphragm material, and the industrial problems that the UHMWPE battery diaphragm is uneven in pore diameter and difficult to prepare are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ultra-high molecular weight nanofibers, and in particular to a method for preparing an ultra-high molecular weight polyethylene nanofiber composite film. Background Art

[0002] At present, commercial lithium battery separators are mostly made of polyethylene (PE), polypropylene (PP) single-layer films or PP / PE / PP multi-layer composite polyolefin microporous materials. Ultra-high molecular weight polyethylene (UHMWPE) separators have become the first choice for new energy vehicle batteries due to their ultra-wear resistance, impact resistance, chemical stability and excellent high and low temperature tolerance. However, UHMWPE separators have problems such as poor melt fluidity and difficult molding and processing.

[0003] The mainstream preparation processes are dry and wet methods. Although the latter has better performance, it is accompanied by complex processes, high costs and environmental risks. Therefore, the commercialization of UHMWPE diaphragms faces challenges in cost, process, quality control and technical barriers, and it is urgent to develop a more stable and economical preparation process.

[0004] Ultra-high molecular weight polyethylene (UHMWPE) has the problems of poor melt fluidity and difficult molding and processing. The preparation of UHMWPE nanofibers has always been an industry problem that is difficult to solve, especially nanofibers with a size below 300nm. The best preparation method at present is to use electrospinning, but most of them are above 500nm. At the same time, this method has low preparation efficiency and high cost.

[0005] In the prior art, the patent with publication number CN102041557B discloses a method for producing high-strength and high-modulus polyethylene fibers, which comprises swelling and dissolving, filtering, spinning, freezing and solidifying, pre-stretching, extraction, drying, super-stretching, and winding, wherein the swelling and dissolving step is carried out in a kneader, and the transparent uniform spinning solution obtained by the swelling and dissolving step is quantitatively fed into a single-screw extruder while stirring for extrusion to obtain high-strength and high-modulus polyethylene fibers. However, the polyethylene fibers prepared by this method are still at the micron level, which greatly limits its application range, and the preparation of ultra-high molecular weight polyethylene nanofibers is still a bottleneck problem.

[0006] In view of this, it is necessary to design an improved method for preparing ultra-high molecular weight polyethylene nanofiber composite membrane to solve the above problems. Summary of the invention

[0007] In view of the defects of the above-mentioned prior art, the purpose of the present invention is to provide a method for preparing an ultra-high molecular weight polyethylene nanofiber composite membrane. The preparation method adopts a method combining sea-island spinning and crystal structure regulation to achieve batch preparation of UHMWPE nanofibers below 300nm, and further refines the UHMWPE fibers by combining multiple regulation effects such as extrusion, stretching and grain refinement of the two components to achieve macro-scale preparation of fiber diameters below 300nm, and then obtains an ultra-high molecular weight polyethylene nanofiber composite membrane with adjustable pore size and thickness through layer-by-layer wet coating technology.

[0008] To achieve the above object, the present invention provides a method for preparing an ultra-high molecular weight polyethylene nanofiber composite membrane, comprising the following steps:

[0009] S1, pre-swelling an ultra-high molecular weight polyethylene powder having a relative average molecular weight of 4.5 million and liquid paraffin in a mass ratio of ultra-high molecular weight polyethylene powder: liquid paraffin = 2:8 to obtain an ultra-high molecular weight polyethylene gel;

[0010] S2, feeding ultra-high molecular weight polyethylene gel, a nucleating agent, and cellulose acetate butyrate into a twin-screw extruder for melt blending and extrusion to obtain a modified gel ultra-high molecular weight polyethylene fiber; the nucleating agent is dibenzylidene sorbitol, di(p-methylbenzylidene) sorbitol, or titanium oxalate;

[0011] S3, soaking the modified gel ultra-high molecular weight polyethylene fiber obtained in step S2 in an acetone solution, extracting the CAB phase and liquid paraffin with acetone to obtain UHMWPE nanofibers with a diameter of less than 300 nm;

[0012] S4, performing hydrophilic modification on the surface of the ultra-high molecular weight polyethylene nanofibers obtained in step S3, and then using a dispersant and a surfactant to disperse the ultra-high molecular weight polyethylene nanofibers of different diameters obtained in step S3 into a stable ultra-high molecular weight polyethylene nanofiber suspension under high-speed shearing;

[0013] S5, using a wet coating process, the suspension obtained in step S4 is coated layer by layer on the surface of a non-woven non-woven fabric, and then the non-woven fabric is removed to obtain an ultra-high molecular weight polyethylene nanofiber composite membrane with adjustable pore size. In step S2, the mass ratio of the ultra-high molecular weight polyethylene, the nucleating agent, and the cellulose acetate butyrate is 20:(0.5-2):(78-79.5).

[0014] Furthermore, the mass concentration of the nucleating agent is 0.5-2.0wt%.

[0015] Furthermore, in step S4, the hydrophilic modification refers to soaking the ultra-high molecular weight polyethylene nanofibers in a sodium permanganate solution.

[0016] Furthermore, in step S4, the dispersant is triethylhexyl phosphoric acid.

[0017] Furthermore, in step S4, the surfactant is sodium alkyl sulfonate.

[0018] Furthermore, the mass fraction of the triethylhexyl phosphoric acid is 2.0wt%-4.0wt%.

[0019] Furthermore, the mass fraction of the sodium alkyl sulfonate is 2.0wt%-4.0wt%.

[0020] The beneficial effects of the present invention are:

[0021] 1. The preparation method of the ultra-high molecular weight polyethylene nanofiber composite membrane provided by the present invention comprises the following steps: firstly, UHMWPE powder is pre-swollen with liquid paraffin (UHMWPE: liquid paraffin=2:8), and then the swollen UHMWPE gel, nucleating agent and CAB are melt-blended by a twin-screw extruder, and the drawing and refinement of UHMWPE in the melt-blending process are achieved by online crystal regulation of UHMWPE during the extrusion process and the stretching and extrusion effect of CAB blending on UHMWPE, and then acetone is used to extract the CAB phase and liquid paraffin to obtain UHMWPE nanofibers, thereby realizing the large-scale preparation of UHMWPE nanofibers with a diameter of less than 300 nm; and then a UHMWPE nanofiber membrane with adjustable pore size and thickness is obtained by a layer-by-layer wet coating technology, which has excellent lyophilicity, a water contact angle of 0, and a tensile strength of 38 MPa, and can be used for battery separator materials (both lyophilicity and tensile properties meet material requirements), thereby solving the industry problem that the pore size of UHMWPE battery separators is uneven and difficult to prepare.

[0022] 2. The present invention uses a nucleating agent such as dibenzylidene sorbitol, di(p-methylbenzylidene) sorbitol or titanium oxalate, and uses the nucleating agent to cause local stress instability, induces the generation of a large number of new crystal nuclei, achieves the purpose of refining the grain size, increasing the number of crystals, and promoting UHMWPE to be easier to draw and the fiber size to be easier to refine. The nucleating agent is preferably titanium oxalate, because when UHMWPE is melted and crystallized, the titanium oxalate surface forms a hydrogen bond with the methylene of UHMWPE as an electron donor, and the molecular chain of the UHMWPE wafer grows more easily on the titanium oxalate surface to form a transcrystalline region between the interfaces, which is more effective in refining the grain size and increasing the number of crystals. Grain refinement enhances the interaction between the molecular chains, making UHMWPE less likely to break after being drawn at a large ratio, and the fiber size is smaller. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a schematic diagram of the process of preparing the ultra-high molecular weight polyethylene nanofiber composite membrane of the present invention.

[0024] Figure 2 This is an electron microscope image of the ultra-high molecular weight polyethylene nanofiber prepared in Example 1.

[0025] Figure 3 This is an electron microscope image of the ultra-high molecular weight polyethylene nanofiber composite membrane prepared in Example 1.

[0026] Figure 4 This is a water contact angle diagram of the ultra-high molecular weight polyethylene nanofiber composite membrane prepared in Example 1.

[0027] Figure 5 This is the tensile stress-strain diagram of the ultra-high molecular weight polyethylene nanofiber composite membrane prepared in Example 1.

[0028] Figure 6 1 is an XRD comparison diagram of the ultra-high molecular weight polyethylene fiber prepared in Example 1 and Comparative Example 1.

[0029] Figure 7 This is an optical microscope comparison of the ultra-high molecular weight polyethylene fibers prepared in Example 1 and Comparative Example 1 after being hot pressed into sheets. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0031] In addition, it should be noted that the terms "comprises", "includes" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or apparatus that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or apparatus.

[0032] See also Figure 1 As shown, the present invention provides a method for preparing an ultra-high molecular weight polyethylene nanofiber composite membrane, comprising the following steps:

[0033] S1, pre-swelling an ultra-high molecular weight polyethylene powder having a relative average molecular weight of 4.5 million and liquid paraffin in a mass ratio of ultra-high molecular weight polyethylene powder: liquid paraffin = 2:8 to obtain an ultra-high molecular weight polyethylene gel;

[0034] S2, feeding ultra-high molecular weight polyethylene gel, nucleating agent and cellulose acetate butyrate into a twin-screw extruder for melt blending and extrusion to obtain modified gel ultra-high molecular weight polyethylene fiber; the nucleating agent is dibenzylidene sorbitol, di(p-methylbenzylidene) sorbitol or titanium oxalate; the melt blending temperature is 220°C, the screw pressure is 2.0-2.2MPa, and the spinneret hole size is 200μm.

[0035] S3, soaking the modified gel ultra-high molecular weight polyethylene fiber obtained in step S2 in an acetone solution, extracting the CAB phase and liquid paraffin with acetone to obtain UHMWPE nanofibers with a diameter of less than 300 nm.

[0036] Wherein, in step S2, the mass ratio of the ultra-high molecular weight polyethylene, the nucleating agent, and the cellulose acetate butyrate is 20:(0.5-2):(78-79.5), preferably 20:1:79.

[0037] The mass concentration of the nucleating agent is 0.5-2.0 wt %, preferably 1.0 wt %.

[0038] S4, performing hydrophilic modification on the surface of the ultra-high molecular weight polyethylene nanofibers obtained in step S3, and then using a dispersant and a surfactant to disperse the ultra-high molecular weight polyethylene nanofibers of different diameters obtained in step S3 into a stable ultra-high molecular weight polyethylene nanofiber suspension under high-speed shearing;

[0039] S5, coating the suspension obtained in step S4 layer by layer on the surface of the non-woven fabric by a wet coating process, and then removing the non-woven fabric to obtain an ultra-high molecular weight polyethylene nanofiber composite membrane with adjustable pore size.

[0040] The hydrophilic modification refers to strong oxidation treatment with sodium permanganate, specifically, soaking the ultra-high molecular weight polyethylene nanofibers obtained in step S3 in a sodium permanganate solution.

[0041] The dispersant is triethylhexyl phosphoric acid, and the mass fraction of triethylhexyl phosphoric acid is 2.0wt%-4.0wt%.

[0042] The surfactant is sodium alkyl sulfonate, and the mass fraction of the sodium alkyl sulfonate is 2.0wt%-4.0wt%.

[0043] The preparation method of the ultra-high molecular weight polyethylene nanofiber composite membrane provided by the present invention is described below with reference to specific embodiments.

[0044] Example 1

[0045] This embodiment provides a method for preparing an ultra-high molecular weight polyethylene nanofiber composite membrane, comprising the following steps:

[0046] S1, pre-swelling an ultra-high molecular weight polyethylene powder having a relative average molecular weight of 4.5 million and liquid paraffin in a mass ratio of ultra-high molecular weight polyethylene powder: liquid paraffin = 2:8 to obtain an ultra-high molecular weight polyethylene gel;

[0047] S2, feeding UHMWPE gel containing 20g solid content, 1g titanium oxalate, and 79g cellulose acetate butyrate into a twin-screw extruder for melt blending and extrusion to obtain modified gel ultra-high molecular weight polyethylene fiber; the melt blending temperature is 220°C, the screw pressure is 2.0-2.2MPa, and the spinneret hole size is 200μm.

[0048] S3, soaking the modified gel ultra-high molecular weight polyethylene fiber obtained in step S2 in an acetone solution, extracting the CAB phase and liquid paraffin with acetone to obtain UHMWPE nanofibers with a diameter of 100-300 nm.

[0049] S4, by hydrophilic modification of the surface of ultra-high molecular weight polyethylene nanofibers (immersion treatment with 1.0wt% sodium permanganate solution for 30min), and then using dispersant triethylhexyl phosphoric acid and surfactant sodium alkyl sulfonate to disperse nanofibers of different diameters into a stable suspension dispersion system under high-speed shearing. The mass fraction of triethylhexyl phosphoric acid is 3.0wt%, and the mass fraction of sodium alkyl sulfonate is 3.0wt%.

[0050] S5, using a spray gun to coat nanofibers of different diameters on the surface of a non-woven polypropylene non-woven fabric three times in succession, and finally removing the polypropylene non-woven fabric to obtain an ultra-high molecular weight polyethylene nanofiber membrane.

[0051] See also Figure 2 , which is an electron microscope image of the UHMWPE nanofibers prepared in Example 1. It can be seen from the image that the average fiber diameter is 266 nm, achieving the large-scale preparation of UHMWPE nanofibers below 300 nm.

[0052] See also Figure 3 , which is an electron microscope image of the ultra-high molecular weight polyethylene nanofiber composite membrane prepared in Example 1. It can be seen from the image that the nanofiber composite membrane has a uniform pore size and the nanofibers are evenly dispersed.

[0053] See also Figure 4 , which is a water contact angle diagram of the ultra-high molecular weight polyethylene nanofiber composite membrane prepared in Example 1. It can be seen that the water contact angle of the ultra-high molecular weight polyethylene nanofiber composite membrane is 0°, indicating that the prepared nanofiber composite membrane has excellent hydrophilic and lyophilic properties.

[0054] See also Figure 5 The figure shows the tensile stress-strain properties of the ultra-high molecular weight polyethylene nanofiber composite membrane prepared in Example 1. It can be seen that the tensile strength of the nanofiber composite membrane can reach 39.6 MPa, indicating that the prepared nanofiber composite membrane has excellent tensile resistance.

[0055] Comparative Example 1

[0056] Comparative Example 1 provides a method for preparing a nanofiber membrane. Compared with Example 1, the difference is that no nucleating agent is added in step S2, and the rest is substantially the same as Example 1, which will not be described herein.

[0057] Figure 6 The XRD comparison diagram of the ultra-high molecular weight polyethylene fiber prepared in Example 1 and Comparative Example 1 shows that the peak intensity of the α-crystal diffraction peak at the position of 17.3° in the diffraction spectrum obtained in Example 1 is significantly increased, indicating that the addition of the nucleating agent titanium oxalate greatly promotes the formation of the α-crystal. According to the Scherrer formula, the grain size becomes smaller and the number increases. That is, the titanium oxalate added in Example 1 makes the UHMWPE wafer more susceptible to the action of interfacial hydrogen bonds, forming a transcrystalline region, greatly refining the grain size, greatly increasing the number of grains, and forming more α-crystals. In Comparative Example 1, the crystal structure shows the XRD spectrum of conventional UHMWPE, and the enhanced α-crystal diffraction peak cannot be obtained, resulting in insufficient drawing ratio in the final UHMWPE melting process and the fiber size cannot reach below 300nm.

[0058] Figure 7 This is an optical microscope comparison of the ultra-high molecular weight polyethylene fiber prepared in Example 1 and Comparative Example 1 after hot pressing into a sheet. It can be seen that compared with the picture without adding a nucleating agent, the number of grains in the microscope picture containing a nucleating agent is greatly increased, and the crystal size is greatly reduced, while the picture without adding a nucleating agent shows a larger grain size and a smaller number of crystals. This once again shows that titanium oxalate can refine the grain size, increase the number of crystals, promote the ultra-high molecular weight polyethylene to be easier to draw, and the fiber size is easier to refine.

[0059] Examples 2-3 and Comparative Example 2

[0060] Examples 2-3 and Comparative Example 2 provide a method for preparing an ultra-high molecular weight polyethylene nanofiber composite membrane, which is different from Example 1 in that the nucleating agent used in step S2 is changed, as shown in Table 1 below, and the remaining steps are substantially the same as Example 1. No further description is given here.

[0061] Table 1

[0062]

[0063] According to Table 1, when the nucleating agent is dibenzylidene sorbitol and di(p-methylbenzylidene) sorbitol, the diameter of the prepared UHMWPE nanofibers is less than 300 nm. This is mainly attributed to the hydrogen bonds formed between dibenzylidene sorbitol and di(p-methylbenzylidene) sorbitol and the surface of UHMWPE, which enhances the shuffle region formed on the surface of UHMWPE on dibenzylidene sorbitol and di(p-methylbenzylidene) sorbitol, effectively increases the drawing ratio of the UHMWPE phase during the melt drawing process, and the fiber size reaches less than 300 nm.

[0064] When no nucleating agent is used, the prepared UHWMPE fibers are larger in size, all larger than 300 nm.

[0065] When the nucleating agent is talcum powder, the prepared UHWMPE fibers are larger in size, all larger than 300 nm.

[0066] The UHMWPE nanofiber composite membranes prepared in Examples 1-3 and Comparative Examples 1-2 were tested, and the results are shown in Table 2.

[0067] Table 2

[0068] Water contact angle (°) Tensile strength(MPa) Example 1 0 39.6 Example 2 0 39.3 Example 3 0 39.2 Comparative Example 1 16 28.7 Comparative Example 2 14 27.5

[0069] Comparing Examples 1-3 with Comparative Example 1, it can be seen that when no nucleating agent is added, the fiber diameter obtained is larger due to the larger size and smaller number of UHMWPE crystals. Compared with the comparative example, the UHMWPE fibers prepared in the examples have a smaller diameter, all less than 300nm, and better fiber strength. The obtained nanofiber composite membrane has excellent hydrophilic and lyophilic properties, and the tensile strength is above 39MPa, which fully meets the performance index requirements of commercial battery separators.

[0070] Comparing Examples 1-3 with Comparative Example 2, it can be seen that when the added nucleating agent is talcum powder, although the size of the obtained UHMWPE fiber is reduced (1000-1500nm), due to the limited regulation of the crystal structure of UHMWPE by talcum powder, the formation effect of UHMWPE nanofibers is not good, the nanofiber size is greater than 1000nm, and the tensile strength of the formed nanofiber composite membrane is reduced to 27.5MPa.

[0071] Examples 4-8 and Comparative Examples 3-4

[0072] The main difference between Examples 4-8 and Comparative Examples 3-4 and Example 1 is that the type of nucleating agent in step S2 and the ratio of the solid content of ultra-high molecular weight polyethylene gel, the nucleating agent, and the cellulose acetate butyrate are changed, as shown in Table 3 below. The rest is roughly the same as Example 1 and will not be repeated here.

[0073] Table 3

[0074]

[0075] The UHMWPE nanofibers prepared in Examples 4-8 and Comparative Examples 3-4 were tested, and the results are shown in Table 4.

[0076] Table 4

[0077]

[0078] According to the above table, for different nucleating agents, the optimal addition amount is 1wt%, and both the fiber strength and modulus are optimal. When the amount of nucleating agent added is too little, the nucleating agent is limited in regulating the crystal structure of UHMWPE, which is mainly manifested in a significant reduction in nucleation sites, a limited number of new crystal nuclei, and a large crystal size with a small number. In Comparative Example 3, since the addition amount of nucleating agent titanium oxalate is only 0.2wt%, the fiber diameter reaches 600-1600nm.

[0079] When the amount of nucleating agent added is too much, the nucleating agent is easy to agglomerate and bond, which greatly reduces the control effect on the UHMWPE crystal, including the limited decrease in grain size and the small increase in the number of grains. In Comparative Example 4, since the amount of nucleating agent titanium oxalate added is 3.0wt%, the fiber diameter reaches 500-1500nm.

[0080] The UHMWPE nanofiber composite membranes prepared in Examples 4-8 and Comparative Examples 3-4 were tested, and the results are shown in Table 5.

[0081] Table 5

[0082] Water contact angle (°) Tensile strength(MPa) Example 4 0 39.3 Example 5 0 39.5 Example 6 0 38.7 Example 7 0 38.5 Example 8 0 38.3 Comparative Example 3 12 36.8 Comparative Example 4 15 36.4

[0083] It can be seen that when the mass concentration of the nucleating agent is 0.5-2.0wt%, the hydrophilic and lyophilic properties of the nanofiber composite membrane are good, the water contact angle is 0°, and the tensile strength does not change much, all above 38MPa. Too little or too much nucleating agent addition will affect the formation of ultra-high molecular weight polyethylene nanofibers, and at the same time, it is not good for the hydrophilic and lyophilic properties of the formed nanofiber membrane, and the tensile properties will also decrease.

[0084] By controlling the spraying process, the pore size can be adjusted; specifically, if the suspension spraying time is shorter, the pore size will be larger; if the spraying time is longer, the fiber distribution will be denser and the pore size will be smaller.

[0085] In summary, the present invention provides a method for preparing an ultra-high molecular weight polyethylene nanofiber composite membrane, firstly, UHMWPE powder is pre-swollen with liquid paraffin (UHMWPE: liquid paraffin = 2:8), then the swollen UHMWPE gel, nucleating agent and CAB are melt-blended by a twin-screw extruder, and the UHMWPE is stretched and refined by online crystal regulation of UHMWPE during the extrusion process and the stretching and extrusion of UHMWPE by CAB blending, and then acetone is used to extract the CAB phase and liquid paraffin to obtain UHMWPE nanofibers, and the macro-scale preparation of UHMWPE nanofibers with a diameter of less than 300nm is achieved, and then the ultra-high molecular weight polyethylene nanofiber composite membrane with adjustable pore size and thickness is obtained by layer-by-layer wet coating technology. The method realizes UHMWPE nanofibers below 300nm by combining sea island spinning and crystal structure regulation, and the obtained composite membrane can be used for battery separator materials, solving the industry problem that the pore size of UHMWPE battery separators is uneven and difficult to prepare.

[0086] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing an ultra-high molecular weight polyethylene nanofiber composite membrane, It is characterized in that The following steps are involved: S1, pre-swelling an ultra-high molecular weight polyethylene powder having a relative average molecular weight of 4.5 million and liquid paraffin in a mass ratio of ultra-high molecular weight polyethylene powder: liquid paraffin = 2:8 to obtain an ultra-high molecular weight polyethylene gel; S2, feeding ultra-high molecular weight polyethylene gel, a nucleating agent, and cellulose acetate butyrate into a twin-screw extruder for melt blending and extrusion to obtain a modified gel ultra-high molecular weight polyethylene fiber; the nucleating agent is dibenzylidene sorbitol, di(p-methylbenzylidene) sorbitol, or titanium oxalate; S3, soaking the modified gel ultra-high molecular weight polyethylene fiber obtained in step S2 in an acetone solution, extracting the CAB phase and liquid paraffin with acetone to obtain UHMWPE nanofibers with a diameter of less than 300 nm; S4, performing hydrophilic modification on the surface of the ultra-high molecular weight polyethylene nanofibers obtained in step S3, and then using a dispersant and a surfactant to disperse the ultra-high molecular weight polyethylene nanofibers of different diameters obtained in step S3 into a stable ultra-high molecular weight polyethylene nanofiber suspension under high-speed shearing; S5, coating the suspension obtained in step S4 layer by layer on the surface of the non-woven fabric by a wet coating process, and then removing the non-woven fabric to obtain an ultra-high molecular weight polyethylene nanofiber composite membrane with adjustable pore size.

2. The method for preparing the ultra-high molecular weight polyethylene nanofiber composite membrane according to claim 1, Features: In step S2, the mass ratio of the ultra-high molecular weight polyethylene, the nucleating agent, and the cellulose acetate butyrate is 20:(0.5-2):(78-79.5).

3. The method for preparing the ultra-high molecular weight polyethylene nanofiber composite membrane according to claim 1, Features: The mass concentration of the nucleating agent is 0.5-2.0 wt %.

4. The method for preparing the ultra-high molecular weight polyethylene nanofiber composite membrane according to claim 1, Features: In step S4, the hydrophilic modification refers to soaking the ultra-high molecular weight polyethylene nanofibers in a sodium permanganate solution.

5. The method for preparing the ultra-high molecular weight polyethylene nanofiber composite membrane according to claim 1, Features: In step S4, the dispersant is triethylhexyl phosphoric acid.

6. The method for preparing the ultra-high molecular weight polyethylene nanofiber composite membrane according to claim 1, Features: In step S4, the surfactant is sodium alkyl sulfonate.

7. The method for preparing the ultra-high molecular weight polyethylene nanofiber composite membrane according to claim 5, Features: The mass fraction of the triethylhexyl phosphoric acid is 2.0 wt%-4.0 wt%.

8. The method for preparing the ultra-high molecular weight polyethylene nanofiber composite membrane according to claim 6, Features: The mass fraction of the sodium alkyl sulfonate is 2.0 wt%-4.0 wt%.