Multi-layer composite floor and preparation method thereof
By using adhesive and fiberglass in the composite floor to closely bond and applying wear-resistant agent to the surface, the problem of insufficient structural strength and wear resistance of the composite floor is solved, and light weight, high strength, wear resistance, aging resistance and The rich colors are suitable for indoor and outdoor scenes.
Patent Information
- Application Number
- CN202411069023.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-19
AI Technical Summary
During the use of existing composite floors, there are problems such as low structural strength, poor wear resistance, poor stability, easy surface wear and easy separation of internal structures, which are difficult to meet the problems of light weight, low thermal expansion and contraction, high strength and resistance. Wear and aging resistance.
By adopting the preparation method of multi-layer composite flooring, by coating adhesive on the surface of the substrate and injecting foam material, tightly bonding the substrate and foam material, combining fiberglass as the substrate, and applying wear-resistant agent on the surface, polyurethane glue is used and aromatic polyurea elastomer materials enhance adhesion and wear resistance.
The multi-layer composite floor is achieved with light weight, high strength, wear resistance, aging resistance and rich colors, avoiding the layering of the floor in hot and cold environments, and improving the applicability of indoor and outdoor applications.
Smart Images

Figure CN118977502A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of composite flooring, and in particular to a multi-layer composite flooring and a preparation method thereof. Background Art
[0002] Flooring is a building material used for the ground or surface of a building, which can beautify the ground or the surface of a building. Wood flooring is highly praised by consumers for its beautiful texture, good heat insulation and sound insulation performance, but the high cost and easy deformation of wood flooring also limit its application range.
[0003] With the increasing market competition and the increasing demand for flooring by consumers, people are constantly looking for high-performance composite flooring. Composite flooring is a type of flooring that has its natural structure artificially changed to achieve certain physical properties. However, the existing composite flooring has the following problems during use: low structural strength, poor wear resistance, poor stability, easy surface wear after long-term use, and easy separation of the internal structure.
[0004] For example, Japanese patent application publication number JP5270899B2 discloses a board material, which includes an appearance part made of a hard foamed polyurethane resin material and a core part made of a metal material and embedded in the appearance part. However, the metal material of the core part of the board material is easily separated from the foamed material of the appearance part, and the product has poor wear resistance and the surface is easily worn.
[0005] Therefore, it is of great practical significance to provide a composite material floor which is light in weight, has low thermal expansion and contraction, high in strength, wear-resistant, aging-resistant and rich in color. Summary of the invention
[0006] In order to solve the above problems, the present invention provides a multi-layer composite floor and a preparation method thereof. The prepared multi-layer composite floor has the properties of light weight, low thermal expansion and contraction, high strength, wear resistance, and aging resistance.
[0007] The technical solution of the present invention to solve the above problems is as follows:
[0008] A method for preparing a multi-layer composite floor comprises the following steps:
[0009] S1, providing a substrate, and coating an adhesive on the surface of the substrate to obtain an adhesive-coated substrate;
[0010] S2, providing a mold, placing the rubber-coated substrate into the mold, and then injecting the foaming material into the mold, curing it, and taking it out of the mold to obtain a coated substrate;
[0011] S3, spraying primer on the surface of the coated substrate, brushing color paint, rubbing color, coating wear-resistant agent, drying, and obtaining the multi-layer composite floor.
[0012] The present invention coats an adhesive on the surface of the substrate and then pours the foaming material, and the substrate and the foaming material are tightly bonded by the adhesive, thereby preventing the floor from being delaminated due to rain, exposure to the sun, etc.; in addition, a wear-resistant agent is coated on the surface of the floor to improve the wear resistance of the floor surface, so that the floor of the present application can be used in outdoor scenes.
[0013] In addition, during the preparation, paints of different colors can be selected as needed, thereby obtaining a multi-layer composite floor with rich colors.
[0014] Preferably, the material of the substrate is selected from at least one of metal and thermosetting synthetic polymer material.
[0015] It is further preferred that the thermosetting synthetic polymer material is glass fiber reinforced plastic. Glass fiber reinforced plastic is composed of a reinforcing material and a resin matrix, and is a fiber-reinforced resin composite material. Among them, the reinforcing material includes glass fiber, carbon fiber, boron fiber, etc., and the resin matrix includes unsaturated polyester, polyurethane, epoxy resin and phenolic resin, etc. Compared with metal, glass fiber reinforced plastic is a lightweight material, and glass fiber reinforced plastic also has high tensile strength and rigidity. Therefore, glass fiber reinforced plastic is a lightweight but strong structural material. In addition, since the matrix of glass fiber reinforced plastic is a resin material, it is easier to bond with an adhesive than a metal material, thereby avoiding the occurrence of floor delamination to the greatest extent.
[0016] Preferably, the adhesive is selected from one or more of polyurethane adhesive, epoxy adhesive and polyolefin adhesive.
[0017] Preferably, the polyurethane adhesive is a two-component polyurethane adhesive.
[0018] Preferably, the two-component polyurethane adhesive comprises a hydroxyl component and an isocyanate component.
[0019] Preferably, the weight ratio of the hydroxyl component to the isocyanate component is (8-12):(1-5).
[0020] More preferably, the hydroxyl component includes polyols, chain extenders, catalysts, and the like.
[0021] The two-component polyurethane adhesive includes a hydroxyl component (polyol, chain extender, catalyst, etc.) and an isocyanate component, which is a reactive adhesive. The two components undergo a cross-linking reaction when mixed to solidify and bond, that is, NCO and OH react to form solid polyurethane, and then the urethane bond, ester bond, and ether bond in the polyurethane are used to form hydrogen bonds and other bonding effects with the polar groups on the surface of the substrate and the foaming material, thereby playing a bonding role. In addition, the NCO group in the polyurethane adhesive can react with the OH group contained in the glass fiber reinforced plastic to form a chemical bonding force, further enhancing the bonding strength between the materials and avoiding the floor stratification phenomenon. The two-component polyurethane adhesive is a solvent-free two-component adhesive, does not contain solvent, will not cause pollution caused by solvent volatilization, and is safe to operate. Because it does not contain solvent itself, it can be directly coated on the substrate without the need for the heating and drying process.
[0022] Preferably, the coating amount of the polyurethane adhesive is (40-60) g / m 2 .
[0023] Preferably, in S2, the temperature of the foaming material is controlled to be 22-32°C.
[0024] Preferably, in S2, the temperature of the mold is controlled to be 35-45° C. and the curing time is 10-20 min.
[0025] Preferably, the foaming material is selected from one or more of polyurethane foaming raw materials, polyolefin foaming raw materials, and polyvinyl chloride foaming raw materials.
[0026] Preferably, the polyurethane foaming raw material comprises components in the following mass ratio: isocyanate component: combined polyether component = (0.9-1.1): (0.9-1.1).
[0027] Preferably, the combined polyether component comprises the following components in parts by weight: 95 to 98 parts of polyether polyol, 1 to 2 parts of tertiary amine, and 1 to 3 parts of surfactant.
[0028] Preferably, the wear-resistant agent is selected from one or more of polyurea coatings, polyurethane coatings, and acrylic coatings.
[0029] Preferably, the coating formed by the polyurea coating contains an aromatic polyurea elastomer.
[0030] The aromatic polyurea elastomer coating comprises an isocyanate component and a polyamine component, wherein the polyamine component comprises a primary amine component and a secondary amine component, and the secondary amine component is an aromatic diamine. Isocyanate component: polyamine component = (0.5-1.5): (0.5-1.5) (molar ratio); the isocyanate component is an MDI semi-prepolymer (NCO mass fraction is between 12% and 15%); the primary amine component: the secondary amine component = (0.2-0.5): (0.5-0.8) (molar ratio); the primary amine component is D-2000, and the secondary amine component is 4,4'-bis(sec-butylamino)-diphenylmethane (MDBA).
[0031] Preferably, the primary amine component:secondary amine component=(0.25-0.35):(0.65-0.75) (molar ratio).
[0032] Among them, the monomer structure formula of D-2000 is:
[0033]
[0034] The structural formula of MDBA is:
[0035]
[0036] The invention also provides a multi-layer composite floor, which is prepared by the preparation method.
[0037] The present invention has the following beneficial effects:
[0038] The present invention applies adhesive between the substrate and the foam material to tightly bond the substrate and the foam material to avoid stratification of the floor in cold and hot environments; further, polyurethane adhesive is selected as adhesive bonding, and glass fiber reinforced plastic is used as the substrate, so that the polyurethane forms hydrogen bonds and other bonding effects with the substrate and the surface of the foam material. In addition, the glass fiber reinforced plastic contains OH groups, wherein the OH on the surface reacts with the NCO in the polyurethane adhesive to form a chemical bonding force, further enhancing the bonding strength between the materials, and the glass fiber reinforced plastic has the characteristics of light weight and high strength, so the multi-layer composite floor prepared with the glass fiber reinforced plastic as the substrate has the characteristics of light weight and high strength; in addition, the present application applies a wear-resistant agent on the surface of the floor to improve the wear resistance of the floor surface, and further selects polyurea coating as a wear-resistant agent. Polyurea is an elastomeric material produced by the chemical reaction of isocyanate and amino compound, which can provide a dense coating film, further enhancing the wear resistance and aging resistance of the floor; in summary, the multi-layer composite floor prepared by the method of the present invention has the characteristics of light weight, low thermal expansion and contraction, high strength, wear resistance, aging resistance, and rich colors, and can be widely used in indoor and outdoor scenes. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] Figure 1 It is a schematic diagram of the partial structure of the multi-layer composite floor in Example 1;
[0040] Figure 2 It is a partial enlarged view of the multi-layer composite floor in Example 1;
[0041] In the figure: 1-glass fiber reinforced plastic, 2-polyurethane glue, 3-polyurethane foaming raw material, 4-paint, 5-polyurea coating. DETAILED DESCRIPTION
[0042] The present invention is further described in detail below based on the accompanying drawings and implementation examples.
[0043] In order to make the purpose, technical scheme and advantages of the present invention more clear, the present invention is further described in detail in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention, rather than all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0044] Example 1
[0045] A method for preparing a multi-layer composite floor comprises the following steps:
[0046] S1, on two 2mm thick fiberglass surfaces according to 50g / m 2 The polyurethane adhesive with a coating amount of 0.2 mm in thickness is applied to obtain two adhesive-coated substrates;
[0047] S2, placing one of the coated substrates into a mold at a temperature of 35°C, pouring the polyurethane foaming raw material into the mold through a foaming pouring machine, and then placing the second coated substrate into another mold, closing the mold, shaking the mold, curing, and taking it out of the mold to obtain a coated substrate, wherein the temperature of the polyurethane foaming raw material is 25°C, the pouring time is 10s, the curing time is 20min, and the curing temperature is 35°C;
[0048] S3, spraying primer on the surface of the coated substrate, brushing color paint, rubbing color, spraying aromatic polyurea elastomer coating to form a coating with a thickness of 0.2 mm, and drying to obtain a multi-layer composite floor.
[0049] In this embodiment:
[0050] The polyurethane adhesive used is a mixture of K-8026 and K-9965 produced by Shanghai Kayouke Adhesive Co., Ltd., wherein the weight ratio of K-8026 to K-9965 is 10:3, K-8026 includes polyol, chain extender, catalyst, etc., and K-9965 includes isocyanate component;
[0051] The polyurethane foaming raw material used comprises the following components in the following weight ratio: isocyanate component: combined polyether component = 1:1, and the combined polyether component comprises the following components in parts by weight: 97 parts of polyether polyol, 2 parts of tertiary amine, and 1 part of surfactant;
[0052] The aromatic polyurea elastomer coating used includes an isocyanate component and a polyamine component, wherein the polyamine component includes a primary amine component and a secondary amine component, and the secondary amine component is an aromatic diamine; in this embodiment, the isocyanate component: the polyamine component = 1.05:1.0 (molar ratio); the isocyanate component is an MDI semi-prepolymer; the primary amine component: the secondary amine component = 0.29:0.71 (molar ratio); the primary amine component is D-2000, and the secondary amine component is MDBA.
[0053] Example 2
[0054] A method for preparing a multi-layer composite floor comprises the following steps:
[0055] S1, on two 2mm thick fiberglass surfaces according to 50g / m 2 The polyurethane adhesive with a coating amount of 0.2 mm in thickness is applied to obtain two adhesive-coated substrates;
[0056] S2, placing one of the coated substrates into a mold at a temperature of 37°C, pouring the polyurethane foaming raw material into the mold through a foaming pouring machine, and then placing the second coated substrate into another mold, closing the mold, shaking the mold, curing, and taking it out from the mold to obtain a coated substrate, wherein the polyurethane foaming raw material temperature is 26°C, the pouring time is 9s, the curing time is 18min, and the curing temperature is 37°C;
[0057] S3, spraying primer on the surface of the coated substrate, brushing color paint, rubbing color, spraying aromatic polyurea elastomer coating to form a coating with a thickness of 0.5 mm, and drying to obtain a multi-layer composite floor.
[0058] In this embodiment:
[0059] The polyurethane adhesive used is a mixture of K-8026 and K-9965 produced by Shanghai Kayouke Adhesive Co., Ltd., wherein the weight ratio of K-8026 to K-9965 is 10:3, K-8026 includes polyol, chain extender, catalyst, etc., and K-9965 includes isocyanate component;
[0060] The polyurethane foaming raw material used comprises the following components in the following weight ratio: isocyanate component: combined polyether component = 1:1, and the combined polyether component comprises the following components in parts by weight: 98 parts of polyether polyol, 1 part of tertiary amine, and 1 part of surfactant;
[0061] The aromatic polyurea elastomer coating used includes an isocyanate component and a polyamine component, wherein the polyamine component includes a primary amine component and a secondary amine component, and the secondary amine component is an aromatic diamine; in this embodiment, the isocyanate component: the polyamine component = 1.05:1.0 (molar ratio); the isocyanate component is an MDI semi-prepolymer; the primary amine component: the secondary amine component = 0.29:0.71 (molar ratio); the primary amine component is D-2000, and the secondary amine component is MDBA.
[0062] Example 3
[0063] A method for preparing a multi-layer composite floor comprises the following steps:
[0064] S1, on two 2mm thick fiberglass surfaces according to 50g / m 2 The polyurethane adhesive with a coating amount of 0.2 mm in thickness is applied to obtain two adhesive-coated substrates;
[0065] S2, placing one of the coated substrates into a mold at a temperature of 39°C, pouring the polyurethane foaming raw material into the mold through a foaming pouring machine, and then placing the second coated substrate into another mold, closing the mold, shaking the mold, curing, and taking it out of the mold to obtain a coated substrate, wherein the polyurethane foaming raw material temperature is 27.5°C, the pouring time is 7s, the curing time is 15min, and the curing temperature is 39°C;
[0066] S3, spraying primer on the surface of the coated substrate, brushing color paint, rubbing color, spraying aromatic polyurea elastomer coating to form a coating with a thickness of 0.5 mm, and drying to obtain a multi-layer composite floor.
[0067] In this embodiment:
[0068] The polyurethane adhesive used is a mixture of K-8026 and K-9965 produced by Shanghai Kayouke Adhesive Co., Ltd., wherein the weight ratio of K-8026 to K-9965 is 10:3, K-8026 includes polyol, chain extender, catalyst, etc., and K-9965 includes isocyanate component;
[0069] The polyurethane foaming raw material used comprises the following components in the following weight ratio: isocyanate component: combined polyether component = 1:1, and the combined polyether component comprises the following components in parts by weight: 97 parts of polyether polyol, 2 parts of tertiary amine, and 1 part of surfactant;
[0070] The aromatic polyurea elastomer coating used includes an isocyanate component and a polyamine component, wherein the polyamine component includes a primary amine component and a secondary amine component, and the secondary amine component is an aromatic diamine; in this embodiment, the isocyanate component: the polyamine component = 1.05:1.0 (molar ratio); the isocyanate component is an MDI semi-prepolymer; the primary amine component: the secondary amine component = 0.29:0.71 (molar ratio); the primary amine component is D-2000, and the secondary amine component is MDBA.
[0071] Example 4
[0072] A method for preparing a multi-layer composite floor comprises the following steps:
[0073] S1, on two 2mm thick fiberglass surfaces according to 50g / m 2 The polyurethane adhesive with a coating amount of 0.2 mm in thickness is applied to obtain two adhesive-coated substrates;
[0074] S2, placing one of the coated substrates into a mold at a temperature of 41°C, pouring the polyurethane foaming raw material into the mold through a foaming pouring machine, and then placing the second coated substrate into another mold, closing the mold, shaking the mold, curing, and taking it out of the mold to obtain a coated substrate, wherein the polyurethane foaming raw material temperature is 27.5°C, the pouring time is 7s, the curing time is 15min, and the curing temperature is 41°C;
[0075] S3, spraying primer on the surface of the coated substrate, brushing color paint, rubbing color, spraying aromatic polyurea elastomer coating to form a coating with a thickness of 0.5 mm, and drying to obtain a multi-layer composite floor.
[0076] In this embodiment:
[0077] The polyurethane adhesive used is a mixture of K-8026 and K-9965 produced by Shanghai Kayouke Adhesive Co., Ltd., wherein the weight ratio of K-8026 to K-9965 is 10:3, K-8026 includes polyol, chain extender, catalyst, etc., and K-9965 includes isocyanate component;
[0078] The polyurethane foaming raw material used comprises the following components in the following weight ratio: isocyanate component: combined polyether component = 1:1, and the combined polyether component comprises the following components in parts by weight: 97 parts of polyether polyol, 2 parts of tertiary amine, and 1 part of surfactant;
[0079] The aromatic polyurea elastomer coating used includes an isocyanate component and a polyamine component, wherein the polyamine component includes a primary amine component and a secondary amine component, and the secondary amine component is an aromatic diamine; in this embodiment, the isocyanate component: the polyamine component = 1.05:1.0 (molar ratio); the isocyanate component is an MDI semi-prepolymer; the primary amine component: the secondary amine component = 0.29:0.71; the primary amine component is D-2000, and the secondary amine component is MDBA.
[0080] Example 5
[0081] A method for preparing a multi-layer composite floor comprises the following steps:
[0082] S1, on two 2mm thick fiberglass surfaces according to 50g / m 2 The polyurethane adhesive with a coating amount of 0.2 mm in thickness is applied to obtain two adhesive-coated substrates;
[0083] S2, placing one of the coated substrates into a mold at a temperature of 45°C, pouring the polyurethane foaming raw material into the mold through a foaming pouring machine, and then placing the second coated substrate into another mold, closing the mold, shaking the mold, curing, and taking it out from the mold to obtain a coated substrate, wherein the polyurethane foaming raw material temperature is 29°C, the pouring time is 5s, the curing time is 13min, and the curing temperature is 45°C;
[0084] S3, spraying primer on the surface of the coated substrate, brushing color paint, rubbing color, spraying aromatic polyurea elastomer coating to form a coating with a thickness of 0.5 mm, and drying to obtain a multi-layer composite floor.
[0085] In this embodiment:
[0086] The polyurethane adhesive used is a mixture of K-8026 and K-9965 produced by Shanghai Kayouke Adhesive Co., Ltd., wherein the weight ratio of K-8026 to K-9965 is 10:3, K-8026 includes polyol, chain extender, catalyst, etc., and K-9965 includes isocyanate component;
[0087] The polyurethane foaming raw material used comprises the following components in the following weight ratio: isocyanate component: combined polyether component = 1:1, and the combined polyether component comprises the following components in parts by weight: 96 parts of polyether polyol, 2 parts of tertiary amine, and 2 parts of surfactant;
[0088] The aromatic polyurea elastomer coating used includes an isocyanate component and a polyamine component, wherein the polyamine component includes a primary amine component and a secondary amine component, and the secondary amine component is an aromatic diamine; in this embodiment, the isocyanate component: the polyamine component = 1.05:1.0 (molar ratio); the isocyanate component is an MDI semi-prepolymer; the primary amine component: the secondary amine component = 0.29:0.71 (molar ratio); the primary amine component is D-2000, and the secondary amine component is MDBA.
[0089] Comparative Example 1
[0090] A method for preparing a multi-layer composite floor comprises the following steps:
[0091] S1. Place a substrate into a mold at a temperature of 41°C, pour a polyurethane foaming raw material into the mold through a foaming pouring machine, and then place another substrate into another mold, close the mold, shake the mold, cure, and take it out of the mold to obtain a coated substrate, wherein the temperature of the polyurethane foaming raw material is 27.5°C, the pouring time is 7s, the curing time is 15min, and the curing temperature is 41°C;
[0092] S2. Spraying primer on the surface of the coated substrate, brushing color paint, rubbing color, spraying aromatic polyurea elastomer coating to form a coating with a thickness of 0.5 mm, and drying to obtain a multi-layer composite floor.
[0093] In this comparative example:
[0094] The polyurethane foaming raw material used comprises the following components in the following weight ratio: isocyanate component: combined polyether component = 1:1, and the combined polyether component comprises the following components in parts by weight: 97 parts of polyether polyol, 2 parts of tertiary amine, and 1 part of surfactant;
[0095] The aromatic polyurea elastomer coating used includes an isocyanate component and a polyamine component, wherein the polyamine component includes a primary amine component and a secondary amine component, and the secondary amine component is an aromatic diamine. In this comparative example, the isocyanate component: the polyamine component = 1.05: 1.0 (molar ratio); the isocyanate component is MDI semi-prepolymer; the primary amine component: the secondary amine component = 0.29: 0.71 (molar ratio); the primary amine component is D-2000, and the secondary amine component is MDBA.
[0096] Comparative Example 2
[0097] A method for preparing a multi-layer composite floor comprises the following steps:
[0098] S1, on two 2mm thick fiberglass surfaces according to 50g / m 2 The polyurethane adhesive with a coating amount of 0.2 mm in thickness is applied to obtain two adhesive-coated substrates;
[0099] S2, placing one of the coated substrates into a mold at a temperature of 41°C, pouring the polyurethane foaming raw material into the mold through a foaming pouring machine, and then placing the second coated substrate into another mold, closing the mold, shaking the mold, curing, and taking it out of the mold to obtain a coated substrate, wherein the polyurethane foaming raw material temperature is 27.5°C, the pouring time is 7s, the curing time is 15min, and the curing temperature is 41°C;
[0100] S3, spraying primer on the surface of the coated substrate, brushing color paint, rubbing color, and drying to obtain the multi-layer composite floor.
[0101] In this comparative example:
[0102] The polyurethane adhesive used is a mixture of K-8026 and K-9965 produced by Shanghai Kayouke Adhesive Co., Ltd., wherein the weight ratio of K-8026 to K-9965 is 10:3, K-8026 includes polyol, chain extender, catalyst, etc., and K-9965 includes isocyanate component;
[0103] The polyurethane foaming raw material used comprises components in the following weight ratio: isocyanate component: combined polyether component = 1:1, and the combined polyether component comprises components in the following weight parts: 97 parts of polyether polyol, 2 parts of tertiary amine, and 1 part of surfactant.
[0104] Comparative Example 3
[0105] A method for preparing a multi-layer composite floor comprises the following steps:
[0106] S1, on two 2mm thick fiberglass surfaces according to 50g / m 2 The polyurethane adhesive with a coating amount of 0.2 mm in thickness is applied to obtain two adhesive-coated substrates;
[0107] S2, placing one of the coated substrates into a mold at a temperature of 41°C, pouring the polyurethane foaming raw material into the mold through a foaming pouring machine, and then placing the second coated substrate into another mold, closing the mold, shaking the mold, curing, and taking it out of the mold to obtain a coated substrate, wherein the temperature of the polyurethane foaming raw material is 20°C, the pouring time is 3s, the curing time is 15min, and the curing temperature is 41°C;
[0108] S3, spraying primer on the surface of the coated substrate, brushing color paint, rubbing color, spraying aromatic polyurea elastomer coating to form a coating with a thickness of 0.5 mm, and drying to obtain a multi-layer composite floor.
[0109] In this comparative example:
[0110] The polyurethane adhesive used is a mixture of K-8026 and K-9965 produced by Shanghai Kayouke Adhesive Co., Ltd., wherein the weight ratio of K-8026 to K-9965 is 10:3, K-8026 includes polyol, chain extender, catalyst, etc., and K-9965 includes isocyanate component;
[0111] The polyurethane foaming raw material used comprises the following components in the following weight ratio: isocyanate component: combined polyether component = 1:1, and the combined polyether component comprises the following components in parts by weight: 97 parts of polyether polyol, 2 parts of tertiary amine, and 1 part of surfactant;
[0112] The aromatic polyurea elastomer coating used includes an isocyanate component and a polyamine component, wherein the polyamine component includes a primary amine component and a secondary amine component, and the secondary amine component is an aromatic diamine; in this comparative example, the isocyanate component: the polyamine component = 1.05:1.0 (molar ratio); the isocyanate component is an MDI semi-prepolymer; the primary amine component: the secondary amine component = 0.29:0.71 (molar ratio); the primary amine component is D-2000, and the secondary amine component is MDBA.
[0113] Comparative Example 4
[0114] A method for preparing a multi-layer composite floor comprises the following steps:
[0115] S1, on two 2mm thick fiberglass surfaces according to 50g / m 2 The polyurethane adhesive with a coating amount of 0.2 mm in thickness is applied to obtain two adhesive-coated substrates;
[0116] S2, placing one of the coated substrates into a mold at a temperature of 41°C, pouring the polyurethane foaming raw material into the mold through a foaming pouring machine, and then placing the second coated substrate into another mold, closing the mold, shaking the mold, curing, and taking it out of the mold to obtain a coated substrate, wherein the polyurethane foaming raw material temperature is 27.5°C, the pouring time is 7s, the curing time is 15min, and the curing temperature is 41°C;
[0117] S3, spraying primer on the surface of the coated substrate, brushing color paint, rubbing color, spraying aromatic polyurea elastomer coating to form a coating with a thickness of 0.5 mm, and drying to obtain a multi-layer composite floor.
[0118] In this comparative example:
[0119] The polyurethane adhesive used is a mixture of K-8026 and K-9965 produced by Shanghai Kayouke Adhesive Co., Ltd., wherein the weight ratio of K-8026 to K-9965 is 10:3, K-8026 includes polyol, chain extender, catalyst, etc., and K-9965 includes isocyanate component;
[0120] The polyurethane foaming raw material used comprises the following components in the following weight ratio: isocyanate component: combined polyether component = 1:1, and the combined polyether component comprises the following components in parts by weight: 97 parts of polyether polyol, 2 parts of tertiary amine, and 1 part of surfactant;
[0121] The aromatic polyurea elastomer coating used includes an isocyanate component and a polyamine component, wherein the polyamine component includes a primary amine component and a secondary amine component, and the secondary amine component is an aromatic diamine; in this comparative example, the isocyanate component: the polyamine component = 1.05:1.0 (molar ratio); the isocyanate component is an MDI semi-prepolymer; the primary amine component: the secondary amine component = 0.9:0.1 (molar ratio); the primary amine component is D-2000, and the secondary amine component is MDBA.
[0122] The performance of Examples 1 to 5 and Comparative Examples 1 to 4 was tested using the following method:
[0123] The density is tested according to ISO 1183-1:2019; the three-point bending performance is tested according to BS EN 15534-1:2014+A1:2017; the linear thermal expansion coefficient is tested according to ASTM D6341-2021; the Shore hardness is tested according to ISO 868:2003; the scratch resistance is tested according to Ford corporate standard; the nail holding force is tested according to BS EN 13446:2002; the moisture content is tested according to ASTM D4442-2020; the thermal cycle is tested according to LY / T 2565-2015; and the UV aging is tested according to ASTM G154-2023.
[0124] Table 1: Performance data table of Examples 1 to 5
[0125]
[0126] Table 2: Performance data table of comparative examples 1 to 4
[0127]
[0128]
[0129] According to the data in Table 1 and Table 2, comparative example 1 has delamination, comparative example 2 has poor scratch resistance and UV aging resistance, comparative example 3 has a larger density, and comparative example 4 has poor scratch resistance and UV aging resistance. Compared with comparative examples 1 to 4, embodiments 1 to 5 have better mechanical properties, are scratch-resistant, and resist UV oxidation, and do not have delamination. This shows that the multi-layer composite floor prepared according to the method of the present invention has the properties of light weight, low thermal expansion and contraction, high strength, wear resistance, and aging resistance.
Claims
1. A method for preparing a multi-layer composite floor, characterized in that: The following steps are involved: S1, providing a substrate, and coating an adhesive on the surface of the substrate to obtain an adhesive-coated substrate; S2, providing a mold, placing the rubber-coated substrate into the mold, and then injecting the foaming material into the mold, curing it, and taking it out of the mold to obtain a coated substrate; S3, spraying primer on the surface of the coated substrate, brushing color paint, rubbing color, coating wear-resistant agent, drying, and obtaining the multi-layer composite floor.
2. The preparation method according to claim 1, characterized in that: The material of the substrate is selected from at least one of metal and thermosetting synthetic polymer material.
3. The preparation method according to claim 1, characterized in that: The adhesive is selected from one or more of polyurethane adhesive, epoxy adhesive and polyolefin adhesive.
4. The preparation method according to claim 3, characterized in that: The polyurethane adhesive is a two-component polyurethane adhesive.
5. The preparation method according to claim 1, characterized in that: In S2, the temperature of the foaming material is controlled to be 22-32°C.
6. The preparation method according to claim 1, characterized in that: In S2, the temperature of the mold is controlled to be 35-45° C. and the curing time is 10-20 min.
7. The preparation method according to claim 1, characterized in that: The foaming material is selected from one or more of polyurethane foaming raw materials, polyolefin foaming raw materials, and polyvinyl chloride foaming raw materials.
8. The preparation method according to claim 1, characterized in that: The wear-resistant agent is selected from one or more of polyurea coatings, polyurethane coatings, and acrylic coatings.
9. The preparation method according to claim 8, characterized in that: The coating formed by the polyurea coating contains an aromatic polyurea elastomer.
10. A multi-layer composite floor, characterized in that: The method is prepared according to any one of claims 1 to 9.
Citation Information
Patent Citations
Polyurethane composite thermal insulation board, manufacturing method and application of the same
CN101220614A
Composite air pipe plate and manufacturing method thereof
CN103909697A
High-strength composite thermal insulation board and preparation method thereof
CN109469217A
Cosmetic material and method for manufacturing cosmetic material
CN111479690A
Glass fiber reinforced polyester antiskid floor and preparation method thereof
CN111572153A