Synthesis method and application of ultrahigh-capacity low-voltage hard carbon

By using ultra-fast heating technology to convert the open pores of hard carbon into closed pores in sodium ion batteries, the problem of insufficient capacity in the platform area of ​​hard carbon materials is solved, and the improvement of high energy density and electrochemical performance is achieved. It is suitable for sodium ions The negative electrode material of the battery.

CN118978141AInactive Publication Date: 2024-11-19XIAMEN UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410930077.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-11
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The application of existing hard carbon materials in sodium ion batteries is limited by their long slope zone characteristics, resulting in insufficient capacity in the platform zone, limiting the energy density and commercial application of the battery.

Method used

The porous carbon source is instantly heated from room temperature to 1500℃-1900℃ under an inert atmosphere under an inert atmosphere at a temperature increase rate of 200℃s-1~1000℃s-1, and continuously heated at the target temperature for 5s-60s and cooled to At room temperature, this ultrafast synthesis technology converts the open pores inside hard carbon into closed pores, improving the richness and electrochemical properties of its internal pore structure.

Benefits of technology

Achieve high platform proportion of hard carbon synthesis, improves the energy density and electrochemical performance of sodium ion batteries, and has the advantages of rapid synthesis, low cost and high efficiency. It is suitable for negative electrode materials for sodium ion, lithium ion and potassium ion batteries. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978141A_ABST
    Figure CN118978141A_ABST
Patent Text Reader

Abstract

The invention discloses a synthesis method and application of ultrahigh-capacity low-voltage hard carbon. The preparation method comprises the following steps: S1, using a heating device to instantly heat a porous carbon source from room temperature to a target temperature of 1500-1900 DEG C at a heating rate of 200-1000 DEG C s <-1 > in an inert atmosphere; then, continuous heating is conducted for 5-60 s at the target temperature; s2, cooling the porous carbon source heated in the step S1 to room temperature to obtain modified hard carbon; the method has the advantages of high synthesis speed, low energy consumption and low cost in the aspect of industrial benefits, hard carbon can be synthesized from cheap porous carbon, and in the aspect of hard carbon structure control, on one hand, open pores which cannot be closed by a traditional tube furnace method can be converted into closed pores, the richness of an internal pore structure of the hard carbon is improved, and on the other hand, the energy consumption is reduced; and on the other hand, accurate regulation and control of the hard carbon microstructure can be realized by using an ultrafast synthesis technology, the size of closed pores in the hard carbon can be accurately controlled, and synthesis of the hard carbon material with high pore utilization rate is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery materials, and in particular to a synthesis method of ultra-high capacity low voltage hard carbon and application thereof. Background Art

[0002] As secondary batteries, lithium-ion batteries have been commercialized in electric vehicles, energy storage and other fields due to their high reversible specific capacity and cycle stability. However, the reserves of lithium resources in the earth are low and expensive, which makes it difficult to meet the growing energy demand in the future. Therefore, it is necessary to develop new energy storage systems. As a new battery system with great potential to replace lithium-ion batteries, sodium-ion batteries have the advantages of high abundance and low cost, which can meet the application needs of large-scale energy storage in the future.

[0003] Hard carbon is considered the most promising negative electrode material for sodium-ion batteries to achieve commercialization due to its wide range of raw material sources, high capacity, low voltage and good electrochemical stability. The characteristic charge and discharge curve of hard carbon materials is characterized by the coexistence of platform and slope regions. As a negative electrode material, the capacity of its platform region determines the capacity of the stable available voltage window in the full battery, which in turn plays a key role in improving the energy density of the full battery. Current hard carbon materials inevitably have a long slope region, which limits their commercial application. Therefore, it is extremely important to develop a hard carbon synthesis strategy with a high platform ratio.

[0004] Based on this, a Chinese patent (CN116443868A) discloses a method for synthesizing high-capacity full-platform hard carbon using Joule heat rapid heating technology. This method achieves the synthesis of high-capacity full-platform hard carbon materials by precisely controlling the internal structure of the hard carbon and constructing a large number of closed-pore structures inside the hard carbon.

[0005] On this basis, further optimization of the synthesis strategy to achieve the synthesis of higher capacity full-platform hard carbon will be conducive to promoting the development of high energy density sodium ion batteries. Therefore, it is desirable in the art to develop a synthesis method for ultra-high capacity, full-platform hard carbon. Summary of the invention

[0006] In view of the problems existing in the above-mentioned prior art, the present invention provides a method for synthesizing ultra-high capacity low-voltage hard carbon and its application, which can effectively solve the problems existing in the above-mentioned prior art.

[0007] The technical solution of the present invention is:

[0008] According to one aspect of the present invention, the steps are as follows:

[0009] S1, using a heating device, the porous carbon source was heated at 200 °C s -1 ~1000℃s -1The heating rate is to instantly heat up from room temperature to the target temperature of 1500℃-1900℃; then, continue heating at the target temperature for 5s-60s;

[0010] S2, cooling the porous carbon source heated in step S1 to room temperature to obtain modified hard carbon.

[0011] Furthermore, in step S1, the heating rate is 1000°C s -1 .

[0012] Furthermore, in step S1, the target temperature is 1600° C., and heating is continued at the target temperature for 20 seconds.

[0013] Furthermore, the porous carbon source comprises one or more of commercial activated carbon, porous carbon and self-made porous carbon, wherein the specific surface area of ​​the porous carbon source is 700-2000m 2 g -1 .

[0014] Furthermore, the heating method of the heating device includes: one or more of plasma spark, Joule heat and microwave heating.

[0015] Furthermore, when the heating device heats the porous carbon source, the atmosphere of the heating device is one or more of vacuum or inert gas.

[0016] According to another aspect of the present invention, an application of modified hard carbon prepared based on any one of the above-mentioned synthesis methods, wherein the modified hard carbon is used as a negative electrode in sodium ion, lithium ion and potassium ion batteries.

[0017] By adopting the above technical solution, the present invention has the following beneficial effects compared with the prior art:

[0018] In terms of industrial benefits, this scheme has the advantages of fast synthesis speed, low energy consumption and low cost. It can synthesize hard carbon from cheap porous carbon. In terms of hard carbon structure control, on the one hand, the open pores that cannot be closed by the traditional tube furnace method can be converted into closed pores, thereby improving the richness of the internal pore structure of hard carbon. On the other hand, the ultrafast synthesis technology can be used to achieve precise regulation of the microstructure of hard carbon, and the size of the closed pores in hard carbon can be precisely controlled to achieve the synthesis of hard carbon materials with high pore utilization. In addition, based on the ultrafast synthesis technology, this method further utilizes the existing microporous structure in porous carbon to achieve the synthesis of hard carbon materials with ultra-high closed pore content. The prepared modified hard carbon has a higher density than the initial material, and at the same time has excellent electrochemical properties, with extremely high platform capacity and charge and discharge efficiency in electrochemical tests. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0020] Figure 1 This is a charge and discharge comparison diagram of sample 1 before and after modification by the present invention;

[0021] Figure 2 This is a charge and discharge comparison diagram of sample 2 before and after modification by the present invention;

[0022] Figure 3 This is a comparison diagram of the charge and discharge curves of starch-based hard carbon with and without etching according to the present invention;

[0023] Figure 4 This is a comparison diagram of the charge and discharge curves of sample 1 before and after modification by microwave heating;

[0024] Figure 5 This is a comparison diagram of the charge and discharge curves of sample 1 of the present invention at different temperatures;

[0025] Figure 6 This is a comparison diagram of the charge and discharge curves of sample 1 of the present invention at different times;

[0026] Figure 7 This is a comparison diagram of the charge and discharge curves of sample 1 of the present invention under normal heating and rapid heating;

[0027] Figure 8 Raman spectra of the original sample 1 and the samples treated at different temperatures;

[0028] Fig. 9 The Raman spectra of sample 1 treated at different times;

[0029] Fig.10 These are the Raman spectra of sample 1 under normal heating and rapid heating. DETAILED DESCRIPTION

[0030] The present invention will be further described in detail below in conjunction with the accompanying drawings and examples. It is particularly noted that the following examples are only used to illustrate the present invention, but are not intended to limit the scope of the present invention. Similarly, the following examples are only partial embodiments of the present invention rather than all embodiments, and all other embodiments obtained by those of ordinary skill in the art without creative work are within the scope of protection of the present invention.

[0031] This scheme provides a method for synthesizing ultra-high capacity low voltage hard carbon, comprising the following steps:

[0032] S1, using a heating device, the porous carbon source was heated at 200 °C s -1 ~1000℃s -1 The heating rate is instantaneously increased from room temperature to a target temperature of 1500°C-1900°C; then, the heating is continued at the target temperature for 5s-60s. The porous carbon source includes one or more of activated carbon, porous carbon and self-made porous carbon, wherein the specific surface area of ​​the porous carbon source is 700-2000m 2 g -1 The heating method of the heating device includes: one or more of plasma spark, Joule heat and microwave heating.

[0033] Preferably, when the heating device heats the porous carbon source, the atmosphere of the heating device is one or more of vacuum or inert gas.

[0034] Preferably, in step S1, the heating rate is 1000°C s -1 ; The target temperature is 1600℃, and heating is continued at the target temperature for 20s.

[0035] S2, cooling the porous carbon source heated in step S1 to room temperature to obtain modified hard carbon.

[0036] Furthermore, the porous carbon source comprises one or more of activated carbon, porous carbon and self-made porous carbon, wherein the specific surface area of ​​the porous carbon source is 700-2000m 2 g -1 .

[0037] Embodiment 1:

[0038] Sample 1 has a specific surface area of ​​800m 2 / g of activated carbon, including but not limited to wood activated carbon, fruit shell activated carbon, coal activated carbon, petroleum activated carbon and regenerated carbon, take 0.5g of sample 1 and place it evenly in the carrier, take the Joule heat device as an example, make sample 1 instantly heat up from room temperature to 1600℃ under inert atmosphere; keep it at 1600℃ for 20s; after the porous carbon source is cooled to room temperature, take it out to obtain modified hard carbon, which is recorded as sample: 1-1600℃-20s. The charge and discharge curves of sample 1 before and after modification are as follows Figure 1 As shown in the figure, it can be seen that by instantaneous heating, the platform capacity of sample 1 increases from 0 to 340 mAh / g, and its specific surface area increases from 800 m 2 / g reduced to 60m 2 / g, indicating that this method can transform a large number of open pores into closed pores, while effectively improving the richness of the internal pore structure of hard carbon, greatly improving its sodium ion storage capacity.

[0039] Embodiment 2:

[0040] Sample 2 has a specific surface area of ​​2000m 2 / g porous carbon, take 0.5g sample 2 and place it evenly in the carrier, take the Joule heat device as an example, and heat sample 1 from room temperature to 1600℃ in an inert atmosphere; keep it at 1600℃ for 20s; take out the porous carbon source after cooling to room temperature to obtain modified hard carbon, which is recorded as: sample 2-1600℃-20s. The charge and discharge curves of sample 2 before and after modification are shown in Figure 2 As shown in the figure, it can be seen that by instantaneous heating, the platform capacity of sample 1 increases from 0 to 250 mAh / g, and its specific surface area increases from 2000 m 2 / g reduced to 150m 2 / g, indicating that this method is also applicable to porous carbon with large specific surface area, and this method has certain universality for porous carbon with different specific surface areas.

[0041] Embodiment 3:

[0042] Sample 3 is starch. Take 100g of starch and add 10g of maleic anhydride to mix and grind evenly. Place it at 80℃ to react for 3h. Take 20g of the obtained product and place it in a small crucible. Pre-carbonize it at 800℃ in a tubular furnace for 3h, during which carbon dioxide is continuously introduced for etching. Take 0.5g of the pre-carbonized starch-derived porous carbon and place it evenly in a carrier. Using a Joule heat device as an example, sample 1 is instantly heated from room temperature to 1600℃ under an inert atmosphere; keep it at 1600℃ for 20s; after the porous carbon source is cooled to room temperature, take it out to obtain modified hard carbon, which is recorded as: starch-CO2-1600℃-20s. The comparison of the charge and discharge curves of sample 3 is shown in the figure below. Figure 3 As shown, it can be seen that the present invention can convert the open pores obtained by carbon dioxide etching into closed pores that can store sodium, thereby increasing the platform capacity.

[0043] Embodiment 4:

[0044] The sample is the same as the sample in Example 1, and is heated by microwave at 1600°C for 20 seconds to obtain modified hard carbon. It is recorded as: Sample 1-microwave heating-1600°C-20 seconds. The charge and discharge curves of Sample 1 before and after modification are as follows: Figure 4 As shown, it can be seen that the present invention is universal in instantaneous heating mode, and microwave heating and Joule heating can achieve similar effects.

[0045] Comparative Example 1:

[0046] The other operation steps of this comparative example 1 are the same as those of the example 1, except that the temperature reaches 1900°C, which is recorded as: sample 1-1900°C-20s. Figure 5 As shown, the original sample, the sample in Example 1 and the sample were subjected to Raman testing, and the obtained Raman spectra were as shown in Figure 8As shown, it can be seen that with the increase of heating temperature, the degree of graphitization of the sample continues to increase, the internal voids continue to increase, the utilization rate decreases, and the platform capacity decreases from 340mAh / g to 200mAh / g.

[0047] Comparative Example 2:

[0048] The other operation steps of this comparative example 2 are the same as those of the example 1, except that the heating time is extended to 2 minutes, which is recorded as: sample 1-1600°C-2 minutes. Figure 6 As shown, the sample in Example 1 and the sample were subjected to Raman testing, and the obtained Raman spectrum was as shown in Fig. 9 As shown, it can be seen that with the increase of heating time, the degree of graphitization of the sample is also increasing, the internal voids are increasing, the utilization rate is decreasing, and the platform capacity is reduced from 340mAh / g to 210mAh / g.

[0049] Comparative Example 3:

[0050] The other operation steps of this comparative example 3 are the same as those of Example 3, except that the starch is pre-carbonized at 800°C for 3h in an argon atmosphere tube furnace instead of being etched with carbon dioxide, which is recorded as: starch-Ar-1600°C-20s. The charge-discharge curves of the sample obtained in Example 3 and this sample are shown in Figure 3 As shown, it can be seen that the platform capacity of the starch-derived hard carbon obtained by CO2 etching increases from 200 mAh / g to 260 mAh / g compared with the starch-derived hard carbon without etching, which illustrates the effectiveness of the present invention in closing the pores of porous carbon, and that the pore closure makes a great contribution to the platform capacity of the hard carbon.

[0051] Comparative Example 4:

[0052] Take 20g of the activated carbon in Example 1, place it in a tube furnace, and heat it to 1600℃ for 3h under argon atmosphere. After cooling, the product is obtained, which is recorded as: Sample 1-Tube Furnace. The charge and discharge curves of this sample and the sample obtained in Example 1 are compared. Figure 7 As shown, the Raman spectra of the two Fig.10 As shown, it can be seen that by replacing the high temperature treatment in the tubular furnace with the instantaneous heating method represented by Joule heat, the instantaneous heating and cooling of Joule heat, the graphitization degree of the porous carbon source is lower than that of the tubular furnace, the number of collapsed and damaged sodium ion storage channels inside the porous carbon source is less, and the internal voids are more abundant. The platform capacity of the obtained porous carbon-derived hard carbon ranges from 130mAh / g to 340mAh / g.

[0053] In addition, the present invention also provides an application of modified hard carbon prepared based on the above synthesis method, and the modified hard carbon is used as a negative electrode for sodium ion, lithium ion and potassium ion batteries.

[0054] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for synthesizing ultra-high capacity low voltage hard carbon, characterized in that: The steps include: S1, using a heating device, the porous carbon source was heated at 200 °C s -1 ~1000℃s -1 The heating rate is to instantly heat up from room temperature to the target temperature of 1500℃-1900℃; then, continue heating at the target temperature for 5s-60s; S2, cooling the porous carbon source heated in step S1 to room temperature to obtain modified hard carbon.

2. The method for synthesizing ultra-high capacity low voltage hard carbon according to claim 1, characterized in that: In step S1, the heating rate is 1000°C s -1 .

3. A method for synthesizing ultra-high capacity low voltage hard carbon as claimed in claim 1 or 2, characterized in that: In the step S1, the target temperature is 1600°C, and heating is continued at the target temperature for 20 seconds.

4. The method for synthesizing ultra-high capacity low voltage hard carbon according to claim 1, characterized in that: The porous carbon source comprises one or more of activated carbon, porous carbon and self-made porous carbon, wherein the specific surface area of ​​the porous carbon source is 700-2000m 2 g -1 .

5. The method for synthesizing ultra-high capacity low voltage hard carbon according to claim 1, characterized in that: The heating method of the heating device includes: one or more of plasma spark, Joule heat and microwave heating.

6. The method for synthesizing ultra-high capacity low voltage hard carbon according to claim 1, characterized in that: When the heating device heats the porous carbon source, the atmosphere of the heating device is one or more of vacuum or inert gas.

7. An application of modified hard carbon prepared by the synthesis method according to any one of claims 1 to 6, characterized in that: The modified hard carbon is used as negative electrode in sodium ion, lithium ion and potassium ion batteries.

Citation Information

Patent Citations

  • Preparation method, application and preparation device of low-voltage and high-specific-capacity hard carbon

    CN116443868A

  • Preparation method of coal-based hard carbon negative electrode material as well as product and application of coal-based hard carbon negative electrode material

    CN117945385A

  • Preparation method of high-efficiency high-specific-capacity soft carbon

    CN118206100A

  • Process for the preparation of thick-walled ceramic products