Molecular sieve with millimeter-scale particle size and preparation method thereof

Through hydrothermal synthesis and segmented crystallization, the problem of difficult to prepare a millimeter-scale silicon-aluminum HZSM-5 molecular sieve in the prior art is solved, and a uniform morphology with a particle size greater than 2mm and a silicon-aluminum HZSM-5 with an open channel is achieved. Molecular sieve simplifies the preparation process and reduces costs, laying the foundation for industrial production.

CN118978170APending Publication Date: 2024-11-19SYNFUELS CHINA TECH CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411202752.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

It is difficult to prepare silicon-aluminum HZSM-5 molecular sieve with a particle size of millimeters in the prior art, and the commonly used solvents are highly toxic, high preparation cost, long crystallization time, and lack an effective industrial production route.

Method used

Using the hydrothermal synthesis route, by optimizing the silicon source and feed ratio, using segmented crystallization method to control grain growth, combined with appropriate silicon-aluminum and template agent ratios, the silicon-aluminum HZSM-5 molecular sieve with a particle size of millimeters is achieved. Prepare without the use of hazardous chemicals.

Benefits of technology

Silicon-aluminum HZSM-5 molecular sieve with a uniform morphology, open pores and controllable size with particle size of more than 2mm was successfully prepared, which simplified the preparation process, reduced costs, and was suitable for host and guest materials in the fields of light, magnetism, electricity, etc.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978170A_ABST
    Figure CN118978170A_ABST
Patent Text Reader

Abstract

The invention provides a silicon-aluminum HZSM-5 molecular sieve with a particle size of millimeter magnitude and a preparation method thereof. The method comprises the following steps: mixing an aluminum source and an aqueous solution of a fluorine-containing mineralizer to obtain a mixed solution 1, and mixing an aqueous solution of an organic template agent and the mixed solution 1 to obtain a mixed solution 2; transferring the mixed solution 2 into a reaction kettle, and adding a seed crystal and a solid silicon source to obtain an initial mixed mother solution; sequentially carrying out first-stage crystallization and second-stage crystallization on the initial mixed mother liquor to obtain ZSM-5 molecular sieve particles; and washing and roasting the ZSM-5 molecular sieve particles to obtain the silicon-aluminum HZSM-5 molecular sieve with the particle size of millimeter magnitude. The silicon-aluminum HZSM-5 molecular sieve provided by the invention does not need ammonium exchange, is uniform in morphology and open in pore channels, and has a wide prospect when being applied to the fields of light, electricity and magnetism as a main body material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the preparation of zeolite molecular sieve materials, and specifically relates to a silicon-aluminum HZSM-5 molecular sieve with a particle size of millimeter order and a preparation method thereof. Background Art

[0002] Using molecular sieve as the main material, pure substances or composite materials as the guest are directed to grow or distribute and arrange in the molecular sieve channels to prepare nanoparticles with controllable microstructures, thereby constructing new nano-host-guest functional materials. This material can be used as information storage materials, optical materials, battery electrodes, chemical sensors, and molecular sieve polymer composite materials. Molecular sieves are the core of the directional design and precision assembly of host-guest nano-functional materials. In order to achieve the orderly distribution, directional arrangement and controllable placement of the guest material, it is not only required that the host molecular sieve exists in the form of a single crystal, but also needs to have an ultra-large grain size to minimize the surface area and avoid irregular arrangement and distribution of the guest material. Therefore, exploring the controllable synthesis route of ultra-large grain molecular sieve materials has become the core and key technical problem that needs to be solved in the promotion and application of host-guest nano-functional materials.

[0003] ZSM-5 molecular sieve is a high-silicon microporous material with unique three-dimensional ten-membered ring cross channels. With its unique channel structure, good separation ability, excellent thermal stability and hydrothermal stability, it has become a very important inorganic porous material and is widely used in many fields such as catalytic cracking, isomerization, alkylation, aromatization, adsorption separation, etc. However, most of the currently published synthetic routes are mainly based on the preparation of small-grained silicon-aluminum HZSM-5 molecular sieves, and there are few reports on the synthetic routes of large-grained or even millimeter-scale silicon-aluminum HZSM-5 molecular sieves.

[0004] CN201310404298.8 discloses a method for preparing a ZSM-5 molecular sieve, and a large-grain ZSM-5 molecular sieve with an average particle size greater than 2 μm is prepared by changing the order of adding the template.

[0005] The synthesis method disclosed in CN201510441006.7 uses different templates to control the growth time of the grains at different temperatures, thereby obtaining HZSM-5 molecular sieves with special morphology and unit cell parameters. Although the molecular sieve shows a higher total olefin yield and propylene yield in the methanol to olefin reaction, the grain size is 10μm.

[0006] CN201711038405.4 discloses a method for preparing a P-ZSM-5 molecular sieve with controllable particle size. By adding alkali metals or surfactants to the synthesis system, a P-ZSM-5 molecular sieve with a particle size of 100 nm to 10 μm is prepared, and the obtained molecular sieve has high hydrothermal stability.

[0007] CN201610056519.0 discloses a solid-state ZSM-5 molecular sieve synthesis method with controllable crystal size, which does not require the addition of water or other solvents, and obtains a ZSM-5 molecular sieve material with a particle size of 1 to 20 μm by adjusting the seed feeding amount.

[0008] The literature (Nature, 1993, 365(6443), 239-242) uses a solvent thermal synthesis route to obtain Dodecasil-3C, Ferrierite, Silicalite and AlPO4 molecular sieve materials with a grain size of the millimeter order. However, pyridine must be used as a solvent, which is highly toxic, and the template agent is relatively expensive, which is not conducive to industrial production.

[0009] From the above patents and research reports, it can be seen that the developed synthetic process route can only obtain micron-sized HZSM-5 molecular sieves. Although there are a few preparation routes for millimeter-sized molecular sieves for other topological structures, there are also problems such as high solvent toxicity, low preparation cost, and long crystallization time (>15 days). Therefore, it is still a big challenge to prepare silicon-aluminum HZSM-5 molecular sieves with a particle size of millimeter level, and there is no route to learn from.

[0010] The present invention optimizes the hydrothermal synthesis route to obtain a silicon-aluminum HZSM-5 molecular sieve with a particle size of the millimeter order and a preparation method thereof. The obtained silicon-aluminum HZSM-5 molecular sieve does not require ammonium exchange and has uniform morphology, open pores and controllable size, laying a foundation for its wide application in the fields of light, magnetism and electricity as a main material in host-guest materials. Summary of the invention

[0011] One of the purposes of the present invention is to provide a method for preparing a silicon-alumina HZSM-5 molecular sieve with a particle size of millimeter order.

[0012] The silicon-alumina HZSM-5 molecular sieve with a particle size of millimeters provided by the present invention is prepared according to a method comprising the following steps:

[0013] 1) mixing an aluminum source and an aqueous solution of a fluorine-containing mineralizer to obtain a mixed solution 1;

[0014] 2) mixing the aqueous solution of the organic template with the mixed solution 1 to obtain a mixed solution 2;

[0015] 3) After the mixed solution 2 is transferred to the reactor, seed crystals and solid silicon source are added to obtain an initial mixed mother solution;

[0016] 4) subjecting the mixed mother liquor to first-stage crystallization and second-stage crystallization in sequence to obtain ZSM-5 molecular sieve particles;

[0017] 5) Washing and calcining the ZSM-5 molecular sieve particles to obtain a silicon-alumina HZSM-5 molecular sieve with a particle size of millimeter order.

[0018] In step 1) of the above method, the aluminum source can be selected from one or more of the following: aluminum sulfate, sodium aluminate, aluminum isopropoxide, pseudo-boehmite, γ-alumina powder (>200 mesh), and aluminum nitrate.

[0019] In step 1) of the above method, the fluorine-containing mineralizer is hydrofluoric acid, ammonium fluoride, or a combination of hydrofluoric acid and ammonium fluoride. - ions and ammonium fluoride - The molar ratio of the ions is 0.01 to 5:1.

[0020] The aluminum source is calculated as Al2O3, and the molar ratio of F- ions in the fluorine-containing mineralizer to Al2O3 in the aluminum source can be 20 to 1000:1, preferably 50 to 500:1, more preferably 100 to 500:1, specifically 200:1, 220:1, 310:1, 350:1, 400:1.

[0021] In step 2) of the above method, the organic template can be selected from one or more of the following: tetrapropylammonium hydroxide, tetrapropylammonium bromide, ethylenediamine, 1-butyl-3-methylimidazolium chloride, n-butylamine, tetraethylammonium hydroxide, tetraethylammonium bromide, preferably tetrapropylammonium hydroxide, tetrapropylammonium bromide, ethylenediamine, 1-butyl-3-methylimidazolium chloride, tetraethylammonium hydroxide.

[0022] The fluorine-containing mineralizer contains F - The molar ratio of the ion to the organic template may be 1 to 20:1, specifically 1:1, 2.0:1, 2.5:1, 3:1, 10:1 or 18:1.

[0023] In step 3) of the above method, the solid silicon source can be selected from at least one of the following: quartz tube, quartz sheet, quartz boat, 10-40 mesh quartz sand, 60-80 mesh quartz sand, quartz powder, preferably quartz tube, quartz sheet, quartz boat, 10-40 mesh quartz sand, 60-80 mesh quartz sand.

[0024] In step 3) of the above method, the seed crystal is a powder molecular sieve with an MFI topological structure, and the SiO2 / Al2O3 molar ratio of the powder molecular sieve with the MFI topological structure can be 30-300:1, preferably 50-300:1, more preferably 65-300:1, specifically 65:1, 100:1, 150:1, 300:1; its particle size can be 50nm-20μm, preferably 100nm-20μm, more preferably 200nm-20μm, specifically 200nm, 500nm, 5μm, 10μm.

[0025] The solid silicon source is calculated as SiO2, and the molar ratio of SiO2 in the solid silicon source to Al2O3 in the aluminum source can be 20 to 2000:1, preferably 100 to 2000:1, more preferably 100 to 1500:1, specifically 100:1, 200:1, 500:1, 600:1, 1000:1, 1500:1.

[0026] The mass ratio of the seed crystal to the solid silicon source is 0.02% to 20%:1, preferably 0.05% to 20%:1, more preferably 0.05% to 15%:1, specifically 0.5%:1, 3%:1, 5%:1, 10%:1.

[0027] In step 4) of the above method, the specific operation of sequentially performing the first stage crystallization and the second stage crystallization on the mixed mother liquor is as follows: under static conditions, the mixed mother liquor is heated to 100-200°C at a heating rate of 0.2-20°C / min for first stage crystallization for 12-72h; then at a turning rate of 10-80r / min, the temperature is increased to 150-230°C at a heating rate of 0.5-5°C / min for second stage crystallization for 84h-240h.

[0028] Preferably, the specific operation of sequentially performing the first stage crystallization and the second stage crystallization on the mixed mother liquor is as follows: under static conditions, heating the mixed mother liquor to 100-190°C at a heating rate of 0.2-20°C / min for first stage crystallization for 18-72h; then heating the mixed mother liquor to 150-220°C at a heating rate of 0.5-2.5°C / min at a turnover rate of 10-70r / min for second stage crystallization for 96h-240h.

[0029] More preferably, the specific operation of sequentially performing the first stage crystallization and the second stage crystallization on the mixed mother liquor is: under static conditions, heating the mixed mother liquor to 100-180°C at a heating rate of 0.5-10°C / min for first stage crystallization for 24-72h; then heating the mixed mother liquor to 180°C-220°C at a heating rate of 0.5-2°C / min at a turnover rate of 10-60r / min for second stage crystallization for 120h-240h.

[0030] Specifically, the specific operation of sequentially performing the first stage crystallization and the second stage crystallization on the mixed mother liquor is as follows: under static conditions, the mixed mother liquor is heated to 150°C at a heating rate of 2.5°C / min for the first stage crystallization for 48 hours; then at a turning rate of 15r / min, the temperature is increased to 180°C at a heating rate of 0.5°C / min for the second stage crystallization for 168 hours.

[0031] The operation of sequentially performing the first stage crystallization and the second stage crystallization on the mixed mother liquor is as follows: under static conditions, the mixed mother liquor is heated to 180° C. at a heating rate of 2.5° C. / min for the first stage crystallization for 48 hours; then, at a tumbling rate of 15 r / min, the temperature is raised to 220° C. at a heating rate of 0.5° C. / min for the second stage crystallization for 168 hours;

[0032] The operation of sequentially performing the first stage crystallization and the second stage crystallization on the mixed mother liquor is as follows: under static conditions, the mixed mother liquor is heated to 120° C. at a heating rate of 0.5° C. / min for the first stage crystallization for 72 hours; then, at a tumbling rate of 20 r / min, the temperature is raised to 220° C. at a heating rate of 1.0° C. / min for the second stage crystallization for 144 hours;

[0033] The operation of sequentially performing the first stage crystallization and the second stage crystallization on the mixed mother liquor is as follows: under static conditions, the mixed mother liquor is heated to 105° C. at a heating rate of 5.0° C. / min for the first stage crystallization for 48 hours; then, at a tumbling rate of 35 r / min, the temperature is raised to 180° C. at a heating rate of 2.0° C. / min for the second stage crystallization for 240 hours;

[0034] The operation of sequentially performing the first stage crystallization and the second stage crystallization on the mixed mother liquor is as follows: under static conditions, the mixed mother liquor is heated to 105° C. at a heating rate of 5.0° C. / min for the first stage crystallization for 48 hours; then, at a tumbling rate of 35 r / min, the temperature is raised to 180° C. at a heating rate of 2.0° C. / min for the second stage crystallization for 120 hours;

[0035] or

[0036] The operation of sequentially performing the first stage crystallization and the second stage crystallization on the mixed mother liquor is as follows: under static conditions, the mixed mother liquor is heated to 105° C. at a heating rate of 5.0° C. / min for the first stage crystallization for 48 hours; then, at a tumbling rate of 35 r / min, the temperature is raised to 180° C. at a heating rate of 2.0° C. / min for the second stage crystallization for 180 hours;

[0037] In step 5) of the above method, the drying temperature is 80 to 150° C. and the drying time is 8 to 24 hours.

[0038] The calcination process is carried out in a tubular furnace, the calcination gas can be one or more of dry air, oxygen or ozone, the gas flow rate is 20-150 mL / min, the temperature is 350-600° C., and the time is 4-48 hours.

[0039] Another object of the present invention is to provide a silicon-aluminum HZSM-5 molecular sieve with a particle size of millimeter order prepared by the above method.

[0040] The silicon-aluminum HZSM-5 molecular sieve has a particle size greater than or equal to 2 mm, and has uniform grain morphology and high crystallinity; meanwhile, the crystallization conditions can be adjusted to prepare HZSM-5 molecular sieve crystals of different particle sizes.

[0041] The particle size of the HZSM-5 molecular sieve may be 2 to 4 mm.

[0042] Compared with the prior art, the present invention adopts a suitable silicon source and feed ratio, adopts different processing conditions in different crystallization processes to control the nucleation and growth process of the molecular sieve, and adopts a segmented crystallization method to control the growth process of the grains at different temperatures, thereby obtaining a silicon-aluminum HZSM-5 molecular sieve with a particle size of more than 3 mm. The preparation method of the super-large grain molecular sieve provided by the present invention is simple, easy to operate, free of hazardous chemicals, and easy to scale up and batch prepare.

[0043] The HZSM-5 molecular sieve with special morphology provided by the present invention can be characterized by the following method:

[0044] (1) Powder X-ray Diffraction (XRD): XRD was used to characterize the physical structure of the obtained sample, and it was determined that the sample was a ZSM-5 molecular sieve with high crystallinity.

[0045] (2) Optical microscope: An optical microscope is used to characterize the morphology of the molecular sieve and visually observe the grain morphology and size.

[0046] (3) Inductively coupled plasma optical emission spectroscopy (ICP-OES): ICP-OES was used to investigate the silicon-to-aluminum ratio of the obtained molecular sieve samples.

[0047] (4) Scanning electron microscopy (SEM): SEM was used to characterize the morphology of the comparative molecular sieve and to visually observe the grain morphology and size. BRIEF DESCRIPTION OF THE DRAWINGS

[0048] Figure 1 This is the XRD spectrum of the HZSM-5 molecular sieve prepared in Example 1.

[0049] Figure 2 This is an optical microscope photograph of the HZSM-5 molecular sieve prepared in Example 1.

[0050] Figure 3 This is an optical microscope photograph of the HZSM-5 molecular sieve prepared in Example 2.

[0051] Figure 4 This is the XRD spectrum of the HZSM-5 molecular sieve prepared in Example 3.

[0052] Figure 5This is an optical microscope photograph of the HZSM-5 molecular sieve prepared in Example 3.

[0053] Figure 6 This is an optical microscope photograph of the HZSM-5 molecular sieve prepared in Example 5.

[0054] Figure 7 This is the XRD spectrum of the HZSM-5 molecular sieve prepared in Example 6.

[0055] Figure 8 This is an optical microscope photograph of the HZSM-5 molecular sieve prepared in Example 6.

[0056] Fig. 9 This is an optical microscope photograph of the HZSM-5 molecular sieve prepared in Example 7.

[0057] Fig.10 This is the XRD spectrum of the HZSM-5 molecular sieve in Comparative Example 1.

[0058] Fig.11 This is the SEM photo of the HZSM-5 molecular sieve in Comparative Example 1.

[0059] Fig.12 This is the XRD spectrum of the HZSM-5 molecular sieve in Comparative Example 2.

[0060] Fig.13 This is the SEM photo of the HZSM-5 molecular sieve in Comparative Example 2. DETAILED DESCRIPTION

[0061] To make the objectives, technical solutions and advantages of the present invention more clear, the present invention will be further described in detail below with reference to the accompanying drawings, but the present invention is not limited thereto.

[0062] Example 1

[0063] A silicon-aluminum molecular sieve with a particle size of millimeters and a preparation method thereof, comprising the following steps:

[0064] Weigh 0.67 18-hydrated aluminum sulfate and add it to 10 g of deionized water. Weigh 14.8 g of ammonium fluoride and add it to 15 g of deionized water. Stir and dissolve completely. Add the aqueous solution of aluminum sulfate to the aqueous solution of ammonium fluoride and mix well. This is called solution A. - The molar ratio of ions to Al2O3 is 400:1; 10.42 g of ethylenediamine is weighed and added into 30 g of deionized water, and stirred to completely dissolve, which is recorded as solution B. -The molar ratio of ions to ethylenediamine organic template is 2.3:1; after adding solution B to solution A and stirring evenly, 1.5g of seed crystals (powdered molecular sieve with MFI topological structure, SiO2 / Al2O3=75, 5μm) are added and fully mixed and then transferred to a 100ml synthesis kettle with a polytetrafluoroethylene liner; 30g of quartz sand with a size of 10 to 40 mesh is weighed as a solid silicon source and added to the synthesis kettle, wherein the molar ratio of SiO2 to Al2O3 in the solid silicon source is 500:1; the synthesis kettle is loaded into a homogeneous reactor, and under static conditions, the temperature is increased to 150°C at a heating rate of 2.5°C / min, and the first stage crystallization is carried out for 48h, and then the temperature is increased to 180°C at a heating rate of 0.5°C / min at a turnover rate of 15r / min for 168h in the second stage crystallization. The product was washed 3 to 5 times, dried at 110° C. for 12 h, and then calcined at 400° C. for 12 h in a 5% O3 / 95% O2 atmosphere with a gas flow rate of 80 mL / min to obtain a large-grained silicon-aluminum HZSM-5 molecular sieve.

[0065] The XRD spectrum of the obtained molecular sieve is attached. Figure 1 , optical photos are attached Figure 2 ;

[0066] From the XRD spectrum, it can be seen that the obtained sample has diffraction peaks belonging to the ZSM-5 molecular sieve (010) crystal plane at 2θ=8.9°, 17.8°, 26.8°, 35.6° and 45.0°. From the optical photograph, it can be seen that the prepared HZSM-5 molecular sieve has a classic "coffin" morphology, and the grain length reaches 2.2mm.

[0067] Example 2

[0068] A silicon-aluminum molecular sieve with a particle size of millimeters and a preparation method thereof, comprising the following steps:

[0069] Weigh 0.34 18-hydrated aluminum sulfate and add it to 10 g of deionized water. Weigh 7.4 g of ammonium fluoride and add it to 15 g of deionized water. Stir and dissolve completely. Add the aqueous solution of aluminum sulfate to the aqueous solution of ammonium fluoride and mix well. This is called solution A. - The molar ratio of ions to Al2O3 is 400:1; 5.21 g of ethylenediamine is weighed and added into 30 g of deionized water, and stirred to completely dissolve, which is recorded as solution B. -The molar ratio of ions to ethylenediamine organic template is 2.3:1; after adding solution B to solution A and stirring evenly, 0.75g of seed crystals (powdered molecular sieve with MFI topological structure, SiO2 / Al2O3=75, 5μm) are added and fully mixed and then transferred to a 100ml synthesis kettle with a polytetrafluoroethylene liner; 15g of quartz sand with a size of 10-40 mesh is weighed and added to the synthesis kettle, wherein the molar ratio of SiO2 to Al2O3 in the solid silicon source is 500:1; the synthesis kettle is loaded into a homogeneous reactor, and under static conditions, the temperature is increased to 150°C at a heating rate of 2.5°C / min, and the first stage crystallization is carried out for 48h, and then the temperature is increased to 180°C at a heating rate of 0.5°C / min at a turning rate of 15r / min for 168h in the second stage crystallization. The product was washed 3 to 5 times, dried at 110° C. for 12 h, and then calcined at 400° C. for 12 h in a 5% O3 / 95% O2 atmosphere with a gas flow rate of 80 mL / min to obtain a large-grained silicon-aluminum HZSM-5 molecular sieve.

[0070] The optical photograph of the obtained molecular sieve is attached. Figure 3 ;

[0071] It can be seen from the optical photographs that the prepared HZSM-5 molecular sieve has a classic "coffin" morphology and the grain length reaches 2.5 mm.

[0072] Example 3

[0073] A silicon-aluminum molecular sieve with a particle size of millimeters and a preparation method thereof, comprising the following steps:

[0074] Weigh 0.34g of aluminum sulfate and add it to 10g of deionized water, weigh 7.4g of ammonium fluoride and add it to 15g of deionized water, stir to dissolve completely, add the aqueous solution of aluminum sulfate to the aqueous solution of ammonium fluoride, and mix evenly, record it as solution A, wherein the molar ratio of F- ion to Al2O3 in ammonium fluoride is 400:1; weigh 5.21g of ethylenediamine and add it to 30g of deionized water, stir to dissolve completely, record it as solution B, wherein the F- ion in ammonium fluoride is 400:1. -The molar ratio of ions to ethylenediamine organic template is 2.3:1; after adding solution B to solution A and stirring evenly, 0.75g of seed crystals (powdered molecular sieve with MFI topological structure, SiO2 / Al2O3=75, 5μm) are added and fully mixed and then transferred to a 100ml synthesis kettle with a polytetrafluoroethylene liner; 15g of quartz sand with a size of 10-40 mesh is weighed and added to the synthesis kettle, wherein the molar ratio of SiO2 to Al2O3 in the solid silicon source is 500:1; the synthesis kettle is loaded into a homogeneous reactor, and under static conditions, the temperature is increased to 180°C at a heating rate of 2.5°C / min, and the first stage crystallization is carried out for 48h, and then the temperature is increased to 220°C at a heating rate of 0.5°C / min at a turnover rate of 15r / min for 168h in the second stage crystallization. The product was washed 3 to 5 times, dried at 110° C. for 12 h, and then calcined at 400° C. for 12 h in a 5% O3 / 95% O2 atmosphere with a gas flow rate of 100 mL / min to obtain a large-grained silicon-aluminum HZSM-5 molecular sieve.

[0075] The XRD spectrum of the obtained molecular sieve is attached. Figure 4 , optical photos are attached Figure 5 ;

[0076] From the XRD spectrum, it can be seen that the obtained sample has diffraction peaks belonging to the ZSM-5 molecular sieve (010) crystal plane at 2θ=8.9°, 17.8°, 26.8°, 35.6° and 45.0°. From the optical photos, it can be seen that the prepared HZSM-5 molecular sieve has a classic "coffin" morphology, and the grain length reaches 3.2mm.

[0077] Example 4

[0078] A silicon-aluminum molecular sieve with a particle size of millimeters and a preparation method thereof, comprising the following steps:

[0079] Weigh 0.52g aluminum nitrate nonahydrate and add it to 12g deionized water, weigh 6.07g hydrofluoric acid (40%) and 4.50g ammonium fluoride and add them to 10g deionized water, stir and dissolve completely to obtain a fluorine-containing mineralizer aqueous solution, add the aluminum nitrate aqueous solution to the fluorine-containing mineralizer aqueous solution, and mix well, which is recorded as solution A, wherein the fluorine in the fluorine-containing mineralizer is - The molar ratio of ions to Al2O3 is 350:1; 14.15 g of 1-butyl-3-methylimidazolium chloride is weighed and added into 40 g of deionized water, and stirred to completely dissolve, which is recorded as solution B. -The molar ratio of ions to 1-butyl-3-methylimidazolium chloride organic template is 3:1; after adding solution B to solution A and stirring evenly, 1.25g of seed crystals (powdered molecular sieve with MFI topological structure, SiO2 / Al2O3=75, 5μm) are added and fully mixed and then transferred to a 100ml synthesis kettle with a polytetrafluoroethylene liner; 25g of quartz sheet is weighed and added to the synthesis kettle, wherein the molar ratio of SiO2 to Al2O3 in the solid silicon source is 600:1; the synthesis kettle is loaded into a homogeneous reactor, and under static conditions, the temperature is increased to 120℃ at a heating rate of 0.5℃ / min, and the first stage crystallization is carried out for 72h, and then the temperature is increased to 220℃ at a heating rate of 1.0℃ / min at a turnover rate of 20r / min for the second stage crystallization for 144h. The product was washed 3 to 5 times, dried at 150°C for 12 h, and then calcined at 400°C for 20 h in an O2 atmosphere with a gas flow rate of 120 mL / min to obtain a large-grained silicon-aluminum HZSM-5 molecular sieve.

[0080] Example 5

[0081] A silicon-aluminum molecular sieve with a particle size of millimeters and a preparation method thereof, comprising the following steps:

[0082] 0.067 g of pseudo-boehmite (dry basis 75%) was added to 15 g of deionized water to obtain a suspension, 3.33 g of hydrofluoric acid (40%) and 1.23 g of ammonium fluoride were added to 12 g of deionized water, and stirred to dissolve completely to obtain a fluorine-containing mineralizer aqueous solution, the pseudo-boehmite suspension was added to the fluorine-containing mineralizer aqueous solution, and mixed evenly, and recorded as solution A, wherein the fluorine in the fluorine-containing mineralizer is 1.23 g. - The molar ratio of ions to Al2O3 is 202:1; 16.27 tetrapropylammonium hydroxide (25%) and 11.78 tetraethylammonium hydroxide (25%) organic templates are weighed and added to 15g deionized water, stirred to completely dissolve, and recorded as solution B, wherein F in the fluorine-containing mineralizer is -The molar ratio of ions to organic templates is 2.8:1; after adding solution B to solution A and stirring evenly, 1.5 g of seed crystals (powdered molecular sieve with MFI topological structure, SiO2 / Al2O3=75, 5 μm) are added and fully mixed and then transferred to a 100 ml synthesis kettle with a polytetrafluoroethylene liner; 30 g of a quartz boat is weighed and added to the synthesis kettle, wherein the molar ratio of SiO2 to Al2O3 in the solid silicon source is 1000:1; the synthesis kettle is loaded into a homogeneous reactor, and under static conditions, the temperature is increased to 105°C at a heating rate of 5.0°C / min, and the first stage crystallization is carried out for 48 hours, and then the temperature is increased to 180°C at a heating rate of 2.0°C / min at a turning rate of 35 r / min for 240 hours in the second stage crystallization. The product was washed 3 to 5 times, dried at 80°C for 24 hours, and then calcined at 500°C for 36 hours in an air atmosphere with a gas flow rate of 100 mL / min to obtain a large-grained silicon-alumina HZSM-5 molecular sieve.

[0083] The optical photograph of the obtained molecular sieve is attached. Figure 5 .

[0084] It can be seen from the optical photographs that the prepared HZSM-5 molecular sieve has a classic "coffin" morphology and the grain length reaches 2.8 mm.

[0085] Example 6

[0086] A silicon-aluminum molecular sieve with a particle size of millimeters and a preparation method thereof, comprising the following steps:

[0087] 0.067 g of pseudo-boehmite (dry basis 75%) was added to 15 g of deionized water to obtain a suspension, 3.33 g of hydrofluoric acid (40%) and 1.23 g of ammonium fluoride were added to 12 g of deionized water, and stirred to dissolve completely to obtain a fluorine-containing mineralizer aqueous solution, the pseudo-boehmite suspension was added to the fluorine-containing mineralizer aqueous solution, and mixed evenly, and recorded as solution A, wherein the fluorine in the fluorine-containing mineralizer is 1.23 g. - The molar ratio of ions to Al2O3 is 202:1; 16.27 tetrapropylammonium hydroxide (25%) and 11.78 tetraethylammonium hydroxide (25%) organic templates are weighed and added to 15g deionized water, stirred to completely dissolve, and recorded as solution B, wherein F in the fluorine-containing mineralizer is -The molar ratio of ions to organic templates is 2.8:1; after adding solution B to solution A and stirring evenly, 4.5 g of seed crystals (powdered molecular sieve with MFI topological structure, SiO2 / Al2O3=75, 5 μm) are added and fully mixed and then transferred to a 100 ml synthesis kettle with a polytetrafluoroethylene liner; 30 g of a quartz boat is weighed and added to the synthesis kettle, wherein the molar ratio of SiO2 to Al2O3 in the solid silicon source is 1000:1; the synthesis kettle is loaded into a homogeneous reactor, and under static conditions, the temperature is raised to 105°C at a heating rate of 5.0°C / min, and the first stage crystallization is carried out for 48 hours, and then the temperature is raised to 180°C at a heating rate of 2.0°C / min at a turning rate of 35 r / min for 120 hours in the second stage crystallization. The product was washed 3 to 5 times, dried at 80°C for 24 hours, and then calcined at 500°C for 36 hours in an air atmosphere with a gas flow rate of 60 mL / min to obtain a large-grained silicon-alumina HZSM-5 molecular sieve.

[0088] The XRD spectrum of the obtained molecular sieve is attached. Figure 7 , optical photos are attached Figure 8 ;

[0089] From the XRD spectrum, it can be seen that the obtained sample has diffraction peaks belonging to the ZSM-5 molecular sieve (010) crystal plane at 2θ=8.9°, 17.8°, 26.8°, 35.6° and 45.0°. From the optical photos, it can be seen that the prepared HZSM-5 molecular sieve has a classic "coffin" morphology, and the grain length reaches 3.2mm.

[0090] Example 7

[0091] A silicon-aluminum molecular sieve with a particle size of millimeters and a preparation method thereof, comprising the following steps:

[0092] 0.067 g of pseudo-boehmite (dry basis 75%) was added to a suspension in 15 g of deionized water, 3.33 g of hydrofluoric acid (40%) and 1.23 g of ammonium fluoride were added to 12 g of deionized water, and stirred to dissolve completely to obtain a fluorine-containing mineralizer aqueous solution. The pseudo-boehmite suspension was added to the fluorine-containing mineralizer aqueous solution and mixed evenly, which was recorded as solution A, wherein the fluorine in the fluorine-containing mineralizer was 1.23 g. - The molar ratio of ions to Al2O3 is 202:1; 16.27 tetrapropylammonium hydroxide (25%) and 11.78 tetraethylammonium hydroxide (25%) organic templates are weighed and added to 15g deionized water, stirred to completely dissolve, and recorded as solution B, wherein F in the fluorine-containing mineralizer is -The molar ratio of ions to organic templates is 2.8:1; after adding solution B to solution A and stirring evenly, 4.5 g of seed crystals (powdered molecular sieve with MFI topological structure, SiO2 / Al2O3=75, 20 μm) are added and fully mixed and then transferred to a 100 ml synthesis kettle with a polytetrafluoroethylene liner; 30 g of a quartz boat is weighed and added to the synthesis kettle, wherein the molar ratio of SiO2 to Al2O3 in the solid silicon source is 1000:1; the synthesis kettle is loaded into a homogeneous reactor, and under static conditions, the temperature is increased to 105°C at a heating rate of 5.0°C / min, and the first stage crystallization is carried out for 48 hours, and then the temperature is increased to 180°C at a heating rate of 2.0°C / min at a turning rate of 35 r / min for 180 hours in the second stage crystallization. The product was washed 3 to 5 times, dried at 80°C for 24 hours, and then calcined at 500°C for 36 hours in an air atmosphere with a gas flow rate of 120 mL / min to obtain a large-grained silicon-alumina HZSM-5 molecular sieve.

[0093] The optical photograph of the obtained molecular sieve is attached. Fig. 9 .

[0094] It can be seen from the optical photographs that the prepared HZSM-5 molecular sieve has a classic "coffin" morphology and the grain length reaches 3.1 mm.

[0095] Comparative Example 1

[0096] The commercially available HZSM-5 (Si / Al=200) molecular sieve of Comparative Example 1 is a product of Tianjin Nanhua Catalyst Co., Ltd., with the trade name NKF-5-200H.

[0097] The XRD spectrum of the molecular sieve is shown in the attached Fig.10 , SEM photos are attached Fig.11 .

[0098] The XRD spectrum shows that the sample has characteristic diffraction peaks belonging to the ZSM-5 molecular sieve. The SEM photo shows that the HZSM-5 molecular sieve grains are stacked and have a length of 5 μm.

[0099] Comparative Example 2

[0100] Weigh 0.067 g of pseudo-boehmite (dry basis 75%) and add it to 15 g of deionized water. Weigh 3.33 g of hydrofluoric acid (40%) and 1.23 g of ammonium fluoride and add them to 12 g of deionized water. Stir and dissolve completely. Add the pseudo-boehmite suspension to the fluorine-containing mineralizer aqueous solution and mix well. This is recorded as solution A. The fluorine-containing mineralizer contains 1.23 g of ammonium fluoride and 0.067 g of pseudo-boehmite. -The molar ratio of ions to Al2O3 is 200:1; 16.27 tetrapropylammonium hydroxide (25%) and 11.78 tetraethylammonium hydroxide (25%) organic templates are weighed and added into 15g deionized water, stirred to completely dissolve, and recorded as solution B, wherein F in the fluorine-containing mineralizer is - The molar ratio of ions to organic templates is 2.5:1; after adding solution B to solution A and stirring evenly, 100g silica sol (SiO2=30wt%) is added under high-speed stirring, fully mixed and transferred to a 200ml synthesis kettle with a polytetrafluoroethylene liner, wherein the molar ratio of SiO2 to Al2O3 in the silicon source is 1000; the synthesis kettle is loaded into a homogeneous reactor, and under static conditions, the temperature is raised to 105℃ at a heating rate of 5.0℃ / min, and the first stage crystallization is carried out for 48h, and then the temperature is raised to 180℃ at a heating rate of 2.0℃ / min at a turnover rate of 35r / min for the second stage crystallization for 120h. The product is washed 3 to 5 times, dried at 80℃ for 24h, and then calcined at 500℃ for 36h in an air atmosphere with a gas flow rate of 80mL / min to obtain a silicon-aluminum HZSM-5 molecular sieve.

[0101] The XRD spectrum of the obtained molecular sieve is attached. Fig.12 , SEM photos are attached Fig.13 ;

[0102] The XRD spectrum shows that the obtained sample has characteristic diffraction peaks belonging to ZSM-5 molecular sieve. The SEM photo shows that the grain length of HZSM-5 molecular sieve is 10.07μm.

[0103] The SiO2 / Al2O3 ratios of the silicon-aluminum HZSM-5 molecular sieves in Examples 1-7 and Comparative Examples 1-2 were measured, and the results are shown below:

[0104] Table 1 SiO2 / Al2O3 ratio of silicon-aluminum HZSM-5 molecular sieves in Examples 1-7 and Comparative Examples 1-2

[0105]

[0106]

[0107] The above is only a preferred embodiment of the present invention. It should be pointed out that ordinary technicians in this technical field can make several improvements and supplements without departing from the method of the present invention. These improvements and supplements should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing HZSM-5 molecular sieve with a particle size of millimeters, comprising: 1) mixing an aluminum source and an aqueous solution of a fluorine-containing mineralizer to obtain a mixed solution 1; 2) mixing the aqueous solution of the organic template with the mixed solution 1 to obtain a mixed solution 2; 3) After the mixed solution 2 is transferred to the reactor, seed crystals and solid silicon source are added to obtain an initial mixed mother solution; 4) subjecting the mixed mother liquor to first-stage crystallization and second-stage crystallization in sequence to obtain ZSM-5 molecular sieve particles; 5) Washing and calcining the ZSM-5 molecular sieve particles to obtain a silicon-alumina HZSM-5 molecular sieve with a particle size of millimeter order.

2. The preparation method according to claim 1, characterized in that: In step 1), the aluminum source can be selected from one or more of the following: aluminum sulfate, sodium aluminate, aluminum isopropoxide, pseudo-boehmite, γ-alumina powder (>200 mesh), aluminum nitrate; the fluorine-containing mineralizer is hydrofluoric acid, ammonium fluoride, or a combination of hydrofluoric acid and ammonium fluoride; the aluminum source is calculated as Al2O3, and F in the fluorine-containing mineralizer is - The molar ratio of ions to Al2O3 in the aluminum source is 20 to 1000:1, preferably 50 to 500:1, more preferably 100 to 500:1, specifically 200:1, 220:1, 310:1, 350:1, 400:

1.

3. The preparation method according to claim 1, characterized in that: In step 2), the organic template can be selected from one or more of the following: tetrapropylammonium hydroxide, tetrapropylammonium bromide, ethylenediamine, 1-butyl-3-methylimidazolium chloride, n-butylamine, tetraethylammonium hydroxide, tetraethylammonium bromide, preferably tetrapropylammonium hydroxide, tetrapropylammonium bromide, ethylenediamine, 1-butyl-3-methylimidazolium chloride, tetraethylammonium hydroxide; the fluorine-containing mineralizer F - The molar ratio of the ion to the organic template may be 1 to 20:1, specifically 1:1, 2.0:1, 2.5:1, 3:1, 10:1 or 18:

1.

4. The preparation method according to claim 1, characterized in that: In step 3), the solid silicon source can be selected from at least one of the following: quartz tube, quartz sheet, quartz boat, 10-40 mesh quartz sand, 60-80 mesh quartz sand, quartz powder, preferably quartz tube, quartz sheet, quartz boat, 10-40 mesh quartz sand, 60-80 mesh quartz sand.

5. The preparation method according to claim 1, characterized in that: In step 3), the seed crystal is a powder molecular sieve with an MFI topological structure, and the SiO2 / Al2O3 molar ratio of the powder molecular sieve with the MFI topological structure can be 30-300:1, preferably 50-300:1, more preferably 65-300:1, specifically 65:1, 100:1, 150:1, 300:1; its particle size can be 50nm-20μm, preferably 100nm-20μm, more preferably 200nm-20μm, specifically 200nm, 500nm, 5μm, 10μm.

6. The preparation method according to claim 1, characterized in that: The solid silicon source is calculated as SiO2, and the molar ratio of SiO2 in the solid silicon source to Al2O3 in the aluminum source can be 20 to 2000:1, preferably 100 to 2000:1, more preferably 100 to 1500:1, specifically 100:1, 200:1, 500:1, 600:1, 1000:1, 1500:

1.

7. The preparation method according to claim 1, characterized in that: The mass ratio of the seed crystal to the solid silicon source is 0.02% to 20%:1, preferably 0.05% to 20%:1, more preferably 0.05% to 15%:1, specifically 0.5%:1, 3%:1, 5%:1, 10%:

1.

8. The preparation method according to claim 1, characterized in that: In step 4), the specific operation of sequentially performing the first stage crystallization and the second stage crystallization on the mixed mother liquor is as follows: under static conditions, the mixed mother liquor is heated to 100-200°C at a heating rate of 0.2-20°C / min for the first stage crystallization for 12-72h; then, at a tumbling rate of 10-80r / min, the temperature is increased to 150-230°C at a heating rate of 0.5-5°C / min for the second stage crystallization for 84h-240h; Preferably, the specific operation of sequentially performing the first stage crystallization and the second stage crystallization on the mixed mother liquor is as follows: under static conditions, the mixed mother liquor is heated to 100-190°C at a heating rate of 0.2-20°C / min for first stage crystallization for 18-72h; then, at a tumbling rate of 10-70r / min, the temperature is increased to 150-220°C at a heating rate of 0.5-2.5°C / min for second stage crystallization for 96h-240h; More preferably, the specific operation of sequentially performing the first stage crystallization and the second stage crystallization on the mixed mother liquor is: under static conditions, heating the mixed mother liquor to 100-180°C at a heating rate of 0.5-10°C / min for first stage crystallization for 24-72h; then heating the mixed mother liquor to 180°C-220°C at a heating rate of 0.5-2°C / min at a turnover rate of 10-60r / min for second stage crystallization for 120h-240h.

9. The preparation method according to claim 1, characterized in that: In step 5), the drying temperature is 80-150°C, and the time is 8-24h; the roasting process is carried out in a tubular furnace, and the roasting gas can be one or more of dry air, oxygen or ozone, the gas flow rate is 20-150mL / min, the temperature is 350-600°C, and the time is 4-48h.

10. A silicon-alumina HZSM-5 molecular sieve with a particle size of millimeter order prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Method for directly preparing HZSM-5 molecular sieve and molding HZSM-5 molecular sieve

    CN105600804A

  • HZSM-5 molecular sieve with nanorod binding structure and preparation method and application of sieve

    CN109354037A

  • Nanometer ZSM-5 molecular sieve aggregate synthesis method

    CN109694087A

  • Millimeter-scale microspheric molecular sieve and preparation method thereof

    CN110655090A

  • Preparation of flaky HZSM-5 molecular sieve catalyst and application of flaky HZSM-5 molecular sieve catalyst in preparation of aromatic hydrocarbon through carbon dioxide hydrogenation

    CN114160183A