Glaze slip for preparing transmutation glaze and preparation method of transmutation glaze

By using glaze slurry and kiln change technology with specific ratios, the problem of uncertainty in color and insufficient performance of the kiln change glaze surface is solved, and the chemical stability, mechanical strength and gloss of the glaze surface are improved. It is suitable for a variety of ceramic products .

CN118978340AActive Publication Date: 2024-11-19JIANGSU GAOCHUN CERAMICS
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411407768.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-10
Publication Date
2024-11-19
Estimated Expiration
2044-10-10

AI Technical Summary

Technical Problem

The existing kiln-changing glaze surface has insufficient color uncertainty and performance during firing, making it difficult to have both chemical stability, mechanical strength and gloss, and it is difficult to achieve ideal color changes during kiln transformation.

Method used

The glaze slurry is prepared in a specific proportion using potassium feldspar, Suzhou soil, quartz, zinc oxide, titanium dioxide, frit, barium carbonate, copper oxide, cobalt oxide and other raw materials, and then sifted finely after ball milling, sprayed on the ceramic blank. The firing temperature is controlled at 1220-1250℃, and the color and gloss of the glaze surface are adjusted by adjusting the calcium content and kiln reaction.

Benefits of technology

It realizes the production of glaze surfaces with specific colors during kiln transformation, improves the chemical stability, mechanical strength and gloss of glaze surfaces. It is suitable for artistic porcelain, craft porcelain and daily tableware, and the thermal stability and safety meet the standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005077146590000021
    Figure BDA0005077146590000021
  • Figure BDA0005077146590000031
    Figure BDA0005077146590000031
  • Figure BDA0005077146590000041
    Figure BDA0005077146590000041
Patent Text Reader

Abstract

The invention discloses glaze slip for preparing a transmutation glaze surface and a preparation method of the transmutation glaze surface. The glaze slip is prepared from the following raw materials in parts by mass: 42 parts of potassium feldspar, 7 parts of Suzhou soil, 5 parts of quartz, 0-8 parts of calcite, 9 parts of zinc oxide, 6.2 parts of titanium dioxide, 25 parts of frit, 7 parts of barium carbonate, 1.4 parts of copper oxide and 2 parts of cobalt oxide. The fineness of the glaze slip reaches 250 meshes, and the specific gravity is 1.5-1.6 g / cm < 3 >. The principle that the opacifying effect of titanium is poor under the condition that the calcium content is low is utilized, and a glaze surface with a transmutation effect is generated through reaction. When the calcium content is moderate, the glaze surface glossiness is good; when the calcium content is low, the glaze surface is poor in glossiness, the glaze surface is matte or even dark, and the color changes to black brown; and the glaze surface is green when the calcium content is high. By controlling the fineness of the glaze slip, the firing quality of the glaze surface is ensured; and by controlling the spraying thickness of the glaze layer, the furnace transmutation effect of the glaze color is ensured. The thermal stability, microwave oven test and lead and cadmium dissolution amount of the product can reach the standard of daily tableware.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a kiln-changed glaze, in particular to a glaze slurry used for preparing the kiln-changed glaze and a preparation method of the kiln-changed glaze, belonging to the technical field of ceramic production. Background Art

[0002] Glaze is a thin layer of glass attached to the surface of ceramic body. It is mainly made of clay, flux materials, barren materials, auxiliary materials and other raw materials through weighing, ball milling, glazing and firing at high temperature. It has the advantages of being dense, hard, shiny and non-absorbent, which greatly improves its service life, and improves the decorativeness of ceramics through rich color changes and special glaze effects.

[0003] The main properties of glaze are:

[0004] 1. Chemical stability: The glaze layer should have a certain resistance to acid and alkali corrosion to prevent the precipitation of heavy metals such as lead and chromium that affect human health. Aluminum oxide and zinc oxide will improve the alkali resistance of the glaze, while calcium oxide, magnesium oxide and barium oxide can effectively improve the chemical stability of the glaze.

[0005] 2. Mechanical strength: Mechanical strength is an important property of glaze. Usually, the ability of glaze to resist tensile stress is many times smaller than its ability to resist compressive stress. Therefore, the glaze must absorb compressive stress instead of tensile stress. This can be achieved by adjusting the expansion coefficient of the body and glaze. The hardness of the glaze is also a very important indicator. Generally, in order to improve the scratch hardness, the content of boron oxide can be reduced, lithium oxide can be used to replace part of potassium oxide, and zinc oxide, barium oxide and magnesium oxide can be used to replace lead oxide.

[0006] 3. Gloss. Gloss is also an important property of glaze. The gloss of glaze is directly related to the refractive index. The larger the refractive index, the stronger the gloss. It can be achieved by reducing the surface tension of the melt and increasing the high-temperature fluidity of the melt.

[0007] Kiln change mainly refers to the uncertain natural changes in the glaze color on the surface of porcelain due to changes in temperature in the kiln during the firing process.

[0008] The goal of ceramic production is to produce a glaze that combines both performance and special colors through kiln firing. Summary of the invention

[0009] In order to solve the deficiencies of the prior art, the object of the present invention is to provide a kiln-changed glaze and a preparation method thereof.

[0010] In order to achieve the above object, the present invention adopts the following technical solution:

[0011] A glaze slurry for preparing a kiln-changed glaze surface, comprising water and raw materials in a mass ratio of 1:1; in parts by mass, the raw materials comprise 42 parts of potassium feldspar, 7 parts of Suzhou soil, 5 parts of quartz, 0-8 parts of calcite, 9 parts of zinc oxide, 6.2 parts of titanium dioxide, 25 parts of frit, 7 parts of barium carbonate, 1.4 parts of copper oxide, and 2 parts of cobalt oxide;

[0012] The chemical composition of the raw materials is:

[0013]

[0014] The glaze slurry has a fineness of 250 mesh and a specific gravity of 1.5-1.6 g / cm 3 .

[0015] The glaze slurry is prepared by:

[0016] According to the mass ratio, the raw material, water and ball are mixed in a ratio of 1:1:1.5. After ball milling, the residue on sieve is 0.07-0.12%.

[0017] A method for preparing a kiln-changed glaze surface comprises spraying the above-mentioned glaze slurry on a ceramic bisque fired body and firing the body to obtain the kiln-changed glaze surface.

[0018] The thickness of the glaze slurry sprayed on the ceramic bisque fired body is 0.5 mm.

[0019] The firing temperature is 1220-1250°C, the high fire is kept warm for 20-30 minutes, the firing time is 5-6 hours, and the firing cycle is 21 hours.

[0020] The method for preparing the kiln-changed glaze also includes pre-firing zinc oxide and titanium dioxide before ball milling, and the pre-firing temperature is 1220-1250°C.

[0021] When the above-mentioned calcite is 0 parts, the kiln-changed glaze surface is black-brown.

[0022] When the above calcite is 4 parts, the kiln-changed glaze is brown.

[0023] When the above calcite is 8 parts, the kiln-changed glaze is green.

[0024] The sintering temperature of the green body is 1200-1250°C, the water absorption rate is 1.5-3.5%, and the chemical composition of the green body is:

[0025]

[0026] The present invention is beneficial in that:

[0027] The invention discloses a glaze slurry for preparing a kiln-changed glaze and a method for preparing a kiln-changed glaze. The glaze is reacted at a melting temperature of 1220-1250°C to produce a brown kiln-changed glaze with a poor opacifying effect when the calcium content is low. The kiln-changed color and effect of titanium are adjusted by changing the calcium content. When the calcium content is moderate, the glaze has good gloss, strong opacifying effect, and the glaze is green. When the calcium content is low, the glaze is matte, the opacifying effect is weak, and the glaze is brown. When the calcium content is zero, the glaze becomes matte and very rough, the opacifying effect is very poor, and the glaze is dark brown. The firing quality of the glaze is ensured by controlling the fineness of the glaze slurry. The kiln-changed effect of the glaze color is ensured by controlling the spraying thickness of the glaze layer and the kiln-changed reaction.

[0028] The kiln-changed glaze surface and the preparation method thereof of the present invention can be used in the firing of artistic porcelain, craft porcelain, and decorative items, and can also be used on daily tableware. The thermal stability, microwave oven test, and lead and cadmium dissolution amount can all meet the standards for daily tableware, and the glaze has strong practicality and wide applicability. DETAILED DESCRIPTION

[0029] The present invention is described in detail below with reference to specific embodiments.

[0030] Example 1

[0031] (1) Preparation of glaze slurry

[0032] ① Weighing: Take 42 parts of feldspar, 7 parts of Suzhou soil, 5 parts of quartz, 4 parts of calcite, 9 parts of zinc oxide, 6.2 parts of titanium dioxide, 25 parts of frit, 7 parts of barium carbonate, 1.4 parts of copper oxide, and 2 parts of cobalt oxide as raw materials for glaze slurry, by weight.

[0033] Among them, zinc oxide and titanium dioxide are pre-calcined before use to remove organic impurities, and the pre-calcination temperature is 1220-1250°C.

[0034] The structure of ceramic products is the internal factor that determines their performance and quality, and the structure of ceramic products is guaranteed by the type of raw materials and the process of production, so the selection of raw materials is particularly important. The chemical composition of the main raw materials selected in the present invention is shown in the following table:

[0035] Chemical composition of glaze raw materials (wt%)

[0036]

[0037] ② Ball milling: According to the ratio of raw materials: ball: water = 1:1.5:1, ball milling is carried out, and then sieved with a 250-mesh sieve. The sieve residue needs to be kept between 0.07-0.12%. The specific gravity of the glaze is 1.5-1.6g / cm 3 .

[0038] (2) Glazing

[0039] First, wipe the body clean with a sponge, and then spray the glaze slurry evenly on the ceramic bisque body, controlling the glaze layer thickness to 0.5mm.

[0040] The blank used in the present invention belongs to stoneware blank (firing temperature 1200-1250° C., water absorption rate 1.5-3.5%). In order to achieve the strength required by dishwashers and meet the use of microwave ovens, the water absorption rate of the blank must be strictly controlled.

[0041] The chemical composition of the blank is shown in the following table:

[0042] Chemical composition of the green body

[0043]

[0044] (3) Firing

[0045] It is fired in an ordinary tunnel kiln with an oxidizing atmosphere, a maximum firing temperature of 1230°C, high fire insulation for 30 minutes, a firing time of 6 hours, and a firing cycle of 21 hours.

[0046] Conclusion: The product obtained by the above process steps has a smooth surface, a brown matte kiln-changed glaze, a warm touch, and a special artistic effect; there are no glaze bubbles on the glaze, and the pinhole rate is less than 1.5%; the thermal stability is good, and the glaze layer does not crack after one heat exchange at 20-200°C; the product strength can adapt to the strong collision of an automatic dishwasher; the lead dissolution of the glaze layer is less than 0.2 mg / L (detection limit), and the cadmium dissolution is less than 0.02 mg / L (detection limit), which is safe for the human body.

[0047] Example 2

[0048] When other conditions remain unchanged, the amount of calcite is changed to 8 parts. The product obtained has a stronger glaze gloss than that of the embodiment and has a bright green kiln-fired effect.

[0049] Example 3

[0050] When all other conditions remain unchanged and the calcite is completely removed, the obtained product will have a dull and rough glaze surface compared to the example, and the color will turn into dark brown.

[0051] Example 4

[0052] When other conditions remain unchanged and the fineness of the glaze slurry is changed to 0.5%, the glaze surface of the obtained product will have pinholes and become rough compared with the example, and the glaze surface quality is also poor.

[0053] When the fineness of the glaze slurry is changed to 0.02%, the product obtained will have glaze shrinkage defects compared with the glaze of the embodiment.

[0054] Example 5

[0055] When other conditions remain unchanged, increasing the thickness of the glaze layer will result in glaze flow defects on the glaze surface of the product produced compared to the glaze surface of Example 1.

[0056] The thickness of the glaze layer is reduced, and the glaze kiln-changing effect of the obtained product is weaker than that of the embodiment.

[0057] From the above embodiments, it can be seen that:

[0058] 1. Influence of raw material components

[0059] The chemical composition of the glaze directly affects the effect of the glaze.

[0060] When the calcium content is moderate, the glaze has good gloss, strong opacifying effect and the glaze is green.

[0061] When the calcium content is lower, the glaze is more matte, the opacifying effect is weaker, and the glaze is brown.

[0062] When the calcium content is zero, the glaze becomes dull and very rough, the opacification effect is very poor, and the glaze is black-brown.

[0063] 2. Influence of glaze slurry fineness

[0064] Fineness has a great influence on the glaze's maturation temperature, high-temperature viscosity, glaze surface quality and crystal size.

[0065] The glaze particles are too coarse, resulting in high viscosity of the glaze at high temperatures, which hinders the discharge of gas and easily forms pinholes or bubbles on the glaze surface. At the same time, the glaze fluidity is also poor, making it difficult to fill the pits left when the gas is discharged from the glaze surface to form pinholes on the glaze surface, and it is not conducive to phase separation crystallization.

[0066] If the glaze is too fine, the glaze will dry more slowly and crack easily, and glaze shrinkage defects will easily occur during firing.

[0067] The invention controls the fineness to be between 0.07% and 0.12% of the residue on the 10,000-hole sieve, which can ensure the quality of the glaze surface and also ensure that the product does not stick to the feet.

[0068] 3. Influence of glaze thickness

[0069] The thickness of the glaze layer has a great influence on the effect of the glaze.

[0070] If the glaze layer is too thick, although the kiln-changing reaction of the glaze surface is stronger, it is easy to produce glaze flow defects;

[0071] If the glaze layer is too thin, although there will be no glaze flow defects, the color of the glaze surface will be lighter and the kiln-changing effect will not be obvious.

[0072] The thickness of the glaze layer is related to the specific gravity of the glaze slurry, the glazing time and the glazing method.

[0073] The specific gravity of the glaze slurry increases, the thickness of the glaze layer is uneven, and it is easy to crack. Too thick a glaze layer may cause glaze flow and shrinkage.

[0074] As the specific gravity of the glaze slurry decreases, the glazing time needs to be extended, and the strength requirements for the body are relatively high.

[0075] The thickness of the glaze layer of the present invention is 0.5 mm, which ensures the kiln-changing effect of the glaze color.

[0076] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the above embodiments do not limit the present invention in any form, and any technical solution obtained by equivalent replacement or equivalent transformation falls within the protection scope of the present invention.

Claims

1. A glaze slurry for preparing kiln-changed glaze, characterized in that: The invention comprises water and raw materials in a mass ratio of 1:1; the raw materials comprise, by mass, 42 parts of potassium feldspar, 7 parts of Suzhou soil, 5 parts of quartz, 0-8 parts of calcite, 9 parts of zinc oxide, 6.2 parts of titanium dioxide, 25 parts of frit, 7 parts of barium carbonate, 1.4 parts of copper oxide, and 2 parts of cobalt oxide; The chemical composition of the raw materials is: The glaze slurry has a fineness of 250 mesh and a specific gravity of 1.5-1.6 g / cm 3 .

2. The glaze slurry according to claim 1, characterized in that: The preparation method is: According to the mass ratio, the raw material, water and ball are mixed in a ratio of 1:1:1.

5. After ball milling, the residue on sieve is 0.07-0.12%.

3. A method for preparing a kiln-changed glaze, characterized in that: The glaze slurry described in claim 1 or 2 is sprayed on a ceramic bisque fired body and fired to obtain a kiln-changed glaze surface.

4. The method for preparing kiln-changed glaze according to claim 3, characterized in that: The thickness of the glaze slurry sprayed on the ceramic bisque fired body is 0.5 mm.

5. The method for preparing kiln-changed glaze according to claim 3, characterized in that: The firing temperature is 1220-1250° C., the high fire is kept warm for 20-30 minutes, the firing time is 5-6 hours, and the firing cycle is 21 hours.

6. The method for preparing kiln-changed glaze according to claim 3, characterized in that: The method also includes pre-firing zinc oxide and titanium dioxide before ball milling, and the pre-firing temperature is 1220-1250°C.

7. The method for preparing kiln-changed glaze according to claim 3, characterized in that: When the calcite is 0 parts, the kiln-changed glaze is dark brown.

8. The method for preparing kiln-changed glaze according to claim 3, characterized in that: When the calcite is 4 parts, the kiln-changed glaze is brown.

9. The method for preparing kiln-changed glaze according to claim 3, characterized in that: When the calcite is 8 parts, the kiln-changed glaze is green.

10. The method for preparing kiln-changed glaze according to claim 3, characterized in that: The sintering temperature of the green body is 1200-1250°C, the water absorption rate is 1.5-3.5%, and the chemical composition of the green body is:

Citation Information

Patent Citations

  • Preparation method of golden red temmku kiln fancy glaze Western-style food dinnerware

    CN102070357A

  • Transmutation glaze material and glazing process

    CN102173873A

  • Preparation method of B2O3-TiO2 series fambe ceramic crystalline glaze

    CN102173875A

  • Yellow matt glaze

    CN109231831A

  • Manufacturing method of copper-series flambed glaze

    CN110342820A