Production process of hollow tempered glass and hollow tempered glass
Through high-temperature tempering treatment and nano-aerogel filling technology, the problem of unstable quality of traditional hollow glass is solved, the impact strength and heat resistance are improved, and high-performance and safe hollowing is achieved through vacuum coating and automated cleaning systems. Tempered glass production.
Patent Information
- Application Number
- CN202410884563.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-03
- Publication Date
- 2024-11-19
AI Technical Summary
In traditional hollow glass production processes, the quality of glass is easily affected by raw materials and processing processes, resulting in unstable quality and affecting the performance and life of the product.
Adopt high-temperature tempering and rapid cooling technology, combined with nano-aerogel filling and secondary sealing technology, enhance the impact strength and heat resistance of the glass, and improve optical performance through vacuum coating to ensure the thermal insulation, sound insulation and airtightness of the glass. .
It significantly improves the impact strength and heat resistance of glass, enhances heat insulation and sound insulation performance, ensures long-term stability and safety of the product, and reduces labor costs and improves service life through automated cleaning systems.
Smart Images

Figure CN118978346A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hollow tempered glass, in particular to a production process of hollow tempered glass and the hollow tempered glass. Background Art
[0002] As users pursue safety and diversity, people have higher and higher requirements for the use of glass. Hollow glass is a glass product that forms a dry gas space between glass layers. It is a new type of building material that has good heat insulation, sound insulation, beautiful and practical, and can reduce the weight of the building. It is made of two or three pieces of glass, using a high-strength and high-airtightness composite adhesive to bond the glass sheets to an aluminum alloy frame containing a desiccant to produce high-efficiency sound insulation and heat insulation glass. Hollow glass has many properties that are superior to ordinary double-layer glass.
[0003] However, most of the glass widely used at present is double-layer flat glass, which has poor impact strength and heat resistance. It is easy to break when impacted and is not safe to use. In addition, under traditional technology, the quality of glass is greatly affected by raw materials and processing technology, and is prone to unstable quality, affecting product performance and life. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention provides a production process for hollow tempered glass and hollow tempered glass, which solves the problem that under traditional processes, the quality of glass is greatly affected by raw materials and processing technology, and is prone to unstable quality, affecting product performance and life.
[0005] To achieve the above objectives, the present invention is implemented through the following technical solutions: A production process of hollow tempered glass, comprising the following steps:
[0006] S1. Raw material selection
[0007] Choose finished glass as raw material to ensure the flatness and purity of the glass surface;
[0008] S2. Cutting and cleaning
[0009] Use a glass cutter to cut the glass according to the designed size. After cutting, use an ultrasonic cleaner to thoroughly clean the glass to remove dust and grease on the surface.
[0010] S3. Edge Processing
[0011] Grind the glass edges with an edge grinder to reduce stress concentration and improve the overall strength of the glass;
[0012] S4.Tempering treatment
[0013] Put the glass into the preheating furnace and slowly heat it to the tempering temperature. After continuous tempering for 6-15 minutes, quickly take the glass out of the furnace and cool it evenly with air to generate uniform compressive stress inside the glass, thereby improving the impact strength and heat resistance of the glass.
[0014] S5. Assemble insulating glass
[0015] Install aluminum alloy or stainless steel spacers between two sheets of glass, fill the spacers with desiccant to prevent water vapor from entering the hollow layer, and then use butyl rubber to make preliminary seals on both sides of the spacers to ensure preliminary airtightness;
[0016] S6. Aerogel filling and secondary sealing
[0017] Fill the nano aerogel into the hollow layer, then distribute it evenly through mechanical vibration or vacuum adsorption, and finally use polysulfide glue or silicone glue for secondary sealing to ensure the long-term stability and sealing of the insulating glass;
[0018] S7. Coating treatment
[0019] Use vacuum coating equipment to coat the glass surface with a low-emissivity film through ion sputtering or evaporation process;
[0020] S8. Inspection and Packaging
[0021] Through thickness measurement, air tightness test and optical performance test, we ensure that the product meets the standards. Then the qualified insulating glass is packaged and the glass corners are protected with shockproof materials to prevent damage during transportation.
[0022] Preferably, the finished glass in S1 is any one of high borosilicate glass, aluminosilicate glass and fused quartz glass.
[0023] Preferably, the tempering temperature in S4 is 620-680° C., and the air pressure in S4 is 0.4-0.8 MPa.
[0024] Preferably, the inert gas in S6 is any one of argon and krypton.
[0025] Preferably, a hollow tempered glass comprises a hollow tempered glass body, an upper convex frame is fixed on the top of the hollow tempered glass body, a screw rod rotates inside the upper convex frame, a micro motor is fixed on the left side of the upper convex frame, and the output end of the micro motor passes through the upper convex frame and is fixedly connected to the screw rod.
[0026] Preferably, the outer diameter thread of the screw rod is connected to a moving block, and the moving block is located in the upper convex frame and slidably connected thereto, a connecting strip is fixed to the bottom of the moving block, connecting rods are provided at both the front and rear ends of the hollow tempered glass body, and the top ends of the connecting rods are fixed to the connecting strips.
[0027] Preferably, cleaning brushes are rotated on the outer diameters of the two connecting rods, and the cleaning brushes are in contact with and slide on the hollow tempered glass body.
[0028] Preferably, a lower convex frame is fixed to the bottom of the hollow tempered glass body, an auxiliary block is slidably arranged inside the lower convex frame, an auxiliary strip is fixed to the top of the auxiliary block, and the top of the auxiliary strip is fixed to the two connecting rods.
[0029] The present invention provides a production process of hollow tempered glass and hollow tempered glass.
[0030] Beneficial effects:
[0031] 1. The present invention generates uniform compressive stress inside the glass by performing a tempering treatment and a rapid cooling process at high temperature, thereby greatly improving the impact strength and heat resistance of the glass and reducing the risk of breakage. The use of air further ensures the uniformity and effect of the cooling process. The nano-aerogel filling makes the hollow layer have better heat insulation and sound insulation properties. At the same time, the secondary sealing ensures long-term air tightness and stability. The coating of the low-emissivity film improves the optical properties of the glass, reduces the penetration of ultraviolet and infrared rays, thereby reducing indoor temperature fluctuations and achieving energy-saving effects.
[0032] 2. The hollow tempered glass finally produced by the production process of the present invention not only has high strength and durability, but also has excellent heat insulation, sound insulation and high optical properties, which can meet the high-demand applications in multiple fields such as construction, transportation, furniture, etc., while ensuring the environmental protection and safety quality of the product.
[0033] 3. The present invention drives the cleaning brush to stick to the glass surface through the connecting rod, and can effectively remove dust and dirt during the movement to ensure the cleaning effect. Due to the joint action of the moving block and the auxiliary block, it is ensured that the pressure applied by the cleaning brush to the glass during the cleaning process is uniform, reducing the risk of scratching or damaging the glass due to uneven pressure. By simply starting the micro motor, the glass surface can be automatically cleaned without complicated operating steps, which is convenient for users to use, reduces the workload of manual cleaning, reduces labor costs, and makes cleaning work safer, especially in high or difficult-to-reach places. Through this efficient and uniform automatic cleaning method, the surface of the hollow tempered glass can be kept clean, and dust and dirt can be prevented from accumulating for a long time, thereby extending the service life of the glass. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 It is a flow chart of the production process of the present invention;
[0035] Figure 2 It is a schematic diagram of the three-dimensional structure of the vacuum tempered glass body in the present invention;
[0036] Figure 3 It is a schematic diagram of the front cross-sectional structure of the upper convex frame in the present invention;
[0037] Figure 4 It is a schematic diagram of the exploded structure of the upper convex frame in the present invention;
[0038] Figure 5 It is a schematic diagram of the exploded structure of the lower convex frame in the present invention.
[0039] Among them, 1. hollow tempered glass body; 2. upper convex frame; 3. micro motor; 4. screw rod; 5. moving block; 6. connecting strip; 7. connecting rod; 8. cleaning brush; 9. lower convex frame; 10. auxiliary block; 11. auxiliary strip. DETAILED DESCRIPTION
[0040] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0041] Embodiment 1:
[0042] like Figure 1 As shown, an embodiment of the present invention provides a production process of hollow tempered glass, comprising the following steps:
[0043] S1. Raw material selection
[0044] Choose finished glass as raw material to ensure the flatness and purity of the glass surface;
[0045] S2. Cutting and cleaning
[0046] Use a glass cutter to cut the glass according to the designed size. After cutting, use an ultrasonic cleaner to thoroughly clean the glass to remove dust and grease on the surface.
[0047] S3. Edge Processing
[0048] Grind the glass edges with an edge grinder to reduce stress concentration and improve the overall strength of the glass;
[0049] S4.Tempering treatment
[0050] Put the glass into the preheating furnace and slowly heat it to the tempering temperature. After tempering for 6 minutes, quickly take the glass out of the furnace and cool it evenly with air to generate uniform compressive stress inside the glass, thereby improving the impact strength and heat resistance of the glass. The number of tempering treatments depends on the actual situation, and can be double or triple tempering treatment to further enhance the impact strength of the glass.
[0051] S5. Assemble insulating glass
[0052] Install aluminum alloy or stainless steel spacers between two sheets of glass, fill the spacers with desiccant to prevent water vapor from entering the hollow layer, and then use butyl rubber to make preliminary seals on both sides of the spacers to ensure preliminary airtightness;
[0053] S6. Aerogel filling and secondary sealing
[0054] Fill the nano aerogel into the hollow layer, then distribute it evenly through mechanical vibration or vacuum adsorption, and finally use polysulfide glue or silicone glue for secondary sealing to ensure the long-term stability and sealing of the insulating glass;
[0055] S7. Coating treatment
[0056] Use vacuum coating equipment to coat the glass surface with a low-emissivity film through ion sputtering or evaporation process;
[0057] S8. Inspection and Packaging
[0058] Through thickness measurement, air tightness test and optical performance test, we ensure that the products meet the standards. Then we pack the qualified insulating glass and use shockproof materials to protect the glass corners to prevent damage during transportation.
[0059] The finished glass in S1 is any one of high borosilicate glass, aluminosilicate glass and fused quartz glass; the tempering temperature in S4 is 620°C, and the air pressure in S4 is 0.4MPa; the inert gas in S6 is any one of argon and krypton.
[0060] By selecting high-quality finished glass such as high borosilicate glass, aluminosilicate glass or fused quartz glass, the high quality of raw materials is ensured, thereby improving the performance of the final product. Advanced glass cutting machines and ultrasonic cleaning machines are used to ensure that the glass size is accurate and the surface is dust-free and grease-free, thereby improving the efficiency and quality of subsequent processing steps. Edge grinding reduces the problem of glass breakage caused by stress concentration and enhances the mechanical strength and safety of the glass. Tempering is carried out at 620°C, and a uniform compressive stress is formed inside the glass through a rapid cooling process, which greatly improves the impact strength and heat resistance of the glass. The use of air further ensures the uniformity and Effect, install a spacer between the two pieces of glass and fill it with desiccant to effectively prevent water vapor from entering and keep the hollow layer dry. At the same time, the initial sealing of butyl rubber ensures the basic airtightness. The filling of nano aerogel and the secondary sealing (using polysulfide glue or silicone glue) technology ensure the long-term stability and excellent thermal insulation performance of the hollow glass. The low-radiation film is added to the glass surface through the vacuum coating process, which significantly improves the heat reflection performance of the glass, thereby improving the energy-saving effect. Through strict thickness measurement, airtightness test and optical performance test, it is ensured that each piece of glass meets the standard requirements. The use of shock-proof material packaging reduces the risk of damage during transportation and ensures the integrity of the product.
[0061] Embodiment 2:
[0062] like Figure 1-5 As shown, an embodiment of the present invention provides a production process of hollow tempered glass, comprising the following steps:
[0063] S1. Raw material selection
[0064] Choose finished glass as raw material to ensure the flatness and purity of the glass surface;
[0065] S2. Cutting and cleaning
[0066] Use a glass cutter to cut the glass according to the designed size. After cutting, use an ultrasonic cleaner to thoroughly clean the glass to remove dust and grease on the surface.
[0067] S3. Edge Processing
[0068] Grind the glass edges with an edge grinder to reduce stress concentration and improve the overall strength of the glass;
[0069] S4.Tempering treatment
[0070] Put the glass into the preheating furnace and slowly heat it to the tempering temperature. After tempering for 15 minutes, quickly take the glass out of the furnace and cool it evenly with air to generate uniform compressive stress inside the glass, thereby improving the impact strength and heat resistance of the glass. The number of tempering treatments depends on the actual situation, and can be double or triple tempering treatments to further enhance the impact strength of the glass.
[0071] S5. Assemble insulating glass
[0072] Install aluminum alloy or stainless steel spacers between two sheets of glass, fill the spacers with desiccant to prevent water vapor from entering the hollow layer, and then use butyl rubber to make preliminary seals on both sides of the spacers to ensure preliminary airtightness;
[0073] S6. Aerogel filling and secondary sealing
[0074] Fill the nano aerogel into the hollow layer, then distribute it evenly through mechanical vibration or vacuum adsorption, and finally use polysulfide glue or silicone glue for secondary sealing to ensure the long-term stability and sealing of the insulating glass;
[0075] S7. Coating treatment
[0076] Use vacuum coating equipment to coat the glass surface with a low-emissivity film through ion sputtering or evaporation process;
[0077] S8. Inspection and Packaging
[0078] Through thickness measurement, air tightness test and optical performance test, we ensure that the products meet the standards. Then we pack the qualified insulating glass and use shockproof materials to protect the glass corners to prevent damage during transportation.
[0079] The finished glass in S1 is any one of high borosilicate glass, aluminosilicate glass and fused quartz glass; the tempering temperature in S4 is 680°C, and the air pressure in S4 is 0.8MPa; the inert gas in S6 is any one of argon and krypton.
[0080] By selecting high-quality finished glass such as high borosilicate glass, aluminosilicate glass or fused quartz glass, the high quality of raw materials is ensured, thereby improving the performance of the final product. Advanced glass cutting machines and ultrasonic cleaning machines are used to ensure that the glass size is accurate and the surface is dust-free and grease-free, thereby improving the efficiency and quality of subsequent processing steps. Edge grinding reduces the problem of glass breakage caused by stress concentration and enhances the mechanical strength and safety of the glass. Tempering is carried out at 680°C, and a uniform compressive stress is formed inside the glass through a rapid cooling process, which greatly improves the impact strength and heat resistance of the glass. The use of air further ensures the uniformity and Effect, install a spacer between the two pieces of glass and fill it with desiccant to effectively prevent water vapor from entering and keep the hollow layer dry. At the same time, the initial sealing of butyl rubber ensures the basic airtightness. The filling of nano aerogel and the secondary sealing (using polysulfide glue or silicone glue) technology ensure the long-term stability and excellent thermal insulation performance of the hollow glass. The low-radiation film is added to the glass surface through the vacuum coating process, which significantly improves the heat reflection performance of the glass, thereby improving the energy-saving effect. Through strict thickness measurement, airtightness test and optical performance test, it is ensured that each piece of glass meets the standard requirements. The use of shock-proof material packaging reduces the risk of damage during transportation and ensures the integrity of the product.
[0081] Embodiment three:
[0082] like Figure 2-5 As shown, an embodiment of the present invention provides a hollow tempered glass, including a hollow tempered glass body 1, an upper convex frame 2 is fixed on the top of the hollow tempered glass body 1, a screw rod 4 is rotated inside the upper convex frame 2, a micro motor 3 is fixed on the left side of the upper convex frame 2, and the output end of the micro motor 3 passes through the upper convex frame 2 and is fixedly connected to the screw rod 4, the outer diameter of the screw rod 4 is threadedly connected to a moving block 5, and the moving block 5 is located in the upper convex frame 2 and is slidably connected thereto, a connecting bar 6 is fixed to the bottom of the moving block 5, connecting rods 7 are provided at the front and rear ends of the hollow tempered glass body 1, and the top ends of the connecting rods 7 are fixed to the connecting bar 6, cleaning brushes 8 are rotated on the outer diameters of the two connecting rods 7, and the cleaning brushes 8 are both attached to and slide with the hollow tempered glass body 1, a lower convex frame 9 is fixed to the bottom of the hollow tempered glass body 1, an auxiliary block 10 is slid inside the lower convex frame 9, an auxiliary bar 11 is fixed to the top of the auxiliary block 10, and the top of the auxiliary bar 11 is fixed to the two connecting rods 7.
[0083] When it is necessary to clean the surface of the hollow tempered glass body 1, the micro motor 2 drives the screw 4 inside the upper convex frame 2 to rotate, so that it drives the moving block 5 to move along the direction of the screw, and the connecting rod 7 moves during the movement of the moving block 5. Therefore, the cleaning brush 8 on the connecting rod 7 will slide along the surface of the hollow tempered glass body 1 with this movement, thereby cleaning the glass surface. In addition, the auxiliary block 10 will also move along with the connecting rod 7 during the moving and cleaning process, so that it can transmit this movement to the bottom end of the connecting rod 7 through the auxiliary strip 11 to ensure that the cleaning brush 8 can move smoothly along the glass surface. Therefore, by moving the connecting rod 7 and because the cleaning brush 8 is close to the glass surface, it can effectively remove dust and dirt on the glass surface during the movement.
[0084] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A production process for hollow tempered glass, characterized in that: The following steps are involved: S1. Raw material selection Choose finished glass as raw material to ensure the flatness and purity of the glass surface; S2. Cutting and cleaning Use a glass cutter to cut the glass according to the designed size. After cutting, use an ultrasonic cleaner to thoroughly clean the glass to remove dust and grease on the surface. S3. Edge Processing Grind the glass edges with an edge grinder to reduce stress concentration and improve the overall strength of the glass; S4.Tempering treatment Put the glass into the preheating furnace and slowly heat it to the tempering temperature. After continuous tempering for 6-15 minutes, quickly take the glass out of the furnace and cool it evenly with air to generate uniform compressive stress inside the glass, thereby improving the impact strength and heat resistance of the glass. S5. Assemble insulating glass Install aluminum alloy or stainless steel spacers between two sheets of glass, fill the spacers with desiccant to prevent water vapor from entering the hollow layer, and then use butyl rubber to make preliminary seals on both sides of the spacers to ensure preliminary airtightness; S6. Aerogel filling and secondary sealing Fill the nano aerogel into the hollow layer, then distribute it evenly through mechanical vibration or vacuum adsorption, and finally use polysulfide glue or silicone glue for secondary sealing to ensure the long-term stability and sealing of the insulating glass; S7. Coating treatment Use vacuum coating equipment to coat the glass surface with a low-emissivity film through ion sputtering or evaporation process; S8. Inspection and Packaging Through thickness measurement, air tightness test and optical performance test, we ensure that the product meets the standards. Then the qualified insulating glass is packaged and the glass corners are protected with shockproof materials to prevent damage during transportation.
2. The production process of hollow tempered glass according to claim 1, characterized in that: The finished glass in S1 is any one of high borosilicate glass, aluminosilicate glass and fused quartz glass.
3. The production process of hollow tempered glass according to claim 1, characterized in that: The tempering temperature in S4 is 620-680° C., and the air pressure in S4 is 0.4-0.8 MPa.
4. The production process of hollow tempered glass according to claim 1, characterized in that: The inert gas in S6 is any one of argon and krypton.
5. A hollow tempered glass, characterized in that: The hollow tempered glass body (1) comprises an upper convex frame (2) fixed on the top of the hollow tempered glass body (1), a screw rod (4) rotating inside the upper convex frame (2), a micro motor (3) fixed on the left side of the upper convex frame (2), and an output end of the micro motor (3) passing through the upper convex frame (2) and fixedly connected to the screw rod (4).
6. The hollow tempered glass according to claim 5, characterized in that: The outer diameter of the screw rod (4) is threadedly connected to a moving block (5), and the moving block (5) is located in the upper convex frame (2) and is slidably connected thereto, a connecting strip (6) is fixed to the bottom of the moving block (5), and connecting rods (7) are provided at both the front and rear ends of the hollow tempered glass body (1), and the top ends of the connecting rods (7) are fixed to the connecting strips (6).
7. The hollow tempered glass according to claim 6, characterized in that: Cleaning brushes (8) are rotatably mounted on the outer diameters of the two connecting rods (7), and the cleaning brushes (8) are in contact with and slide against the hollow tempered glass body (1).
8. The hollow tempered glass according to claim 6, characterized in that: A lower convex frame (9) is fixed at the bottom of the hollow tempered glass body (1), an auxiliary block (10) is slidably mounted inside the lower convex frame (9), an auxiliary strip (11) is fixed at the top of the auxiliary block (10), and the top of the auxiliary strip (11) is fixed to the two connecting rods (7).
Citation Information
Cited By
Low-spontaneous-explosion body energy-saving series glass and preparation method thereof
CN119874185A