Foam concrete as well as preparation method and application thereof

By using nanofoam, ultrafine filler and polyvinyl alcohol fiber in foam concrete, the problem of reduced strength of foam concrete is solved, and the characteristics of low volume and high strength are achieved, the scope of application is broadened, and the material is improved Durability and fire resistance.

CN118978366APending Publication Date: 2024-11-19UNIV OF MACAU +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411041878.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

While reducing the density of existing foam concrete, the strength is greatly reduced, making it difficult to take into account both the low volume and high strength.

Method used

Nanofoam, ultrafine filler and polyvinyl alcohol fiber are used to adjust the raw material ratio and mixing process to improve the hydration speed and tensile performance, and combine the nanofoam to reduce the density to form foam concrete with low volume and high strength.

Benefits of technology

It achieves the improvement of the compressive and flexural strength of foam concrete while low volume weight, reduces water absorption and thermal conductivity, broadens the scope of application, and improves the durability and fire resistance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004972587630000071
    Figure BDA0004972587630000071
  • Figure BDA0004972587630000081
    Figure BDA0004972587630000081
  • Figure BDA0004972587630000082
    Figure BDA0004972587630000082
Patent Text Reader

Abstract

The invention discloses foam concrete as well as a preparation method and application thereof, and belongs to the technical field of concrete materials. The foam concrete provided by the invention is prepared from the following raw materials in parts by mass: 500 to 1200 parts of cementing material, 10 to 800 parts of superfine filler, 1 to 30 parts of polyvinyl alcohol fiber and 100 to 800 parts of water, the raw materials further comprise nano-foam, and the volume ratio of the nano-foam to the cementing material is (0.05-30): 1; and the particle size range of the superfine filling material is 1-50 [mu] m. By adding the nano-foam, the cementing material, the superfine filler and the polyvinyl alcohol fiber, the hydration time of the foam concrete is effectively shortened, the compressive strength and the breaking strength of the foam concrete are improved, meanwhile, the percentage of close area in the foam concrete is increased, the water absorption rate and the thermal conductivity of the foam concrete are effectively reduced, and the foam concrete has a good application prospect. The foam concrete with low volume weight and high strength is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of concrete materials, and in particular relates to foamed concrete and a preparation method and application thereof. Background Art

[0002] Foamed concrete is a microporous lightweight material made by mechanically foaming a pre-prepared foaming agent, adding the foam to the cementitious material to reduce the weight, mixing evenly, pouring and curing. Its outstanding feature is the foam holes formed in the concrete, which make the high-density cement concrete lightweight and functional, thus giving the concrete various functions such as lightweight, heat preservation, heat insulation, sound insulation, fire prevention, and corrosion resistance. While the density is reduced, its strength is greatly reduced, and with the continuous increase in the amount of foam, its slow setting problem is also continuously magnified. Therefore, how to solve the problem that the strength of foamed concrete is greatly reduced while reducing the bulk density is now the focus of research. Summary of the invention

[0003] In order to overcome at least one of the problems existing in the above-mentioned prior art, one of the objectives of the present invention is to provide a foamed concrete which can maintain good strength while reducing its bulk density.

[0004] A second object of the present invention is to provide a method for preparing the above-mentioned foamed concrete.

[0005] A third object of the present invention is to provide an application of the foamed concrete.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is:

[0007] The first aspect of the present invention provides a foamed concrete, comprising the following raw materials in parts by mass: 500 to 1200 parts of cementitious material, 10 to 800 parts of ultrafine filler, 1 to 30 parts of polyvinyl alcohol fiber, and 100 to 800 parts of water; the raw materials also include nano foam, and the volume ratio of the nano foam to the cementitious material is (0.05 to 30): 1; the particle size range of the ultrafine filler is 1 to 50 μm.

[0008] The inventive concept of the present invention is as follows: the ultrafine filler used in the present invention has a smaller particle size and low hydration heat, and can play a good filling and reinforcing role. The combination of the cementitious material and the ultrafine filler increases the hydration speed, makes the hydration more complete, and promotes the generation of a large number of hydration products. A large number of hydration products are filled in the pores and bonded to each other, so that microcracks and porosity are reduced, thereby improving the strength of the foamed concrete; the polyvinyl alcohol fiber has high tensile properties, and can ensure the tensile properties of the foamed concrete under the condition of low dry density; the nano foam reduces the bulk density of the concrete, giving the concrete the characteristics of light weight and high compressive strength. The foamed concrete obtained by the combination of various raw materials in the present invention has the characteristics of low bulk density and high strength.

[0009] Preferably, in the foamed concrete, the particle size of the ultrafine filler is in the range of 8 to 45 μm; more preferably, in the range of 15 to 40 μm; and even more preferably, in the range of 20 to 35 μm.

[0010] In some specific embodiments of the present invention, the particle size range of the ultrafine filler refers to the particle size range of the ultrafine filler. 90 Particle size refers to the maximum particle size value corresponding to 90% of the cumulative distribution from small to large in the particle size distribution.

[0011] Preferably, in the foamed concrete, the particle size of the cementitious material is in the range of 1 to 40 μm; more preferably, in the range of 8 to 35 μm; and even more preferably, in the range of 15 to 30 μm.

[0012] In some specific embodiments of the present invention, the particle size range of the gelling material refers to the particle size range of the gelling material. 90 Particle size refers to the maximum particle size value corresponding to 90% of the cumulative distribution from small to large in the particle size distribution.

[0013] Furthermore, the present invention uses ultrafine cementitious materials with small particle sizes. The ultrafine cementitious materials with small particle sizes have the characteristics of fast hydration and high strength. When combined with ultrafine fillers, they have better hydration effects and are beneficial to improving the strength of foam concrete.

[0014] Preferably, in the foamed concrete, the specific surface area of ​​the cementitious material is ≥550m 2 / kg; more preferably 550 to 2000m 2 / kg.

[0015] Preferably, in the foamed concrete, the cementitious material is selected from cement; further preferably, the cement is selected from Portland cement.

[0016] Preferably, in the foamed concrete, the mass fraction of the cementitious material is 550 to 1100 parts; more preferably, it is 600 to 1000 parts; and even more preferably, it is 650 to 800 parts.

[0017] Preferably, in the foamed concrete, the ultrafine filler includes mineral powder and / or fly ash; further preferably, the ultrafine filler includes mineral powder and fly ash.

[0018] Preferably, in the foamed concrete, the mass fraction of the ultrafine filler is 30 to 700 parts; more preferably, it is 60 to 600 parts; and even more preferably, it is 150 to 450 parts.

[0019] Preferably, in the foamed concrete, the aspect ratio of the polyvinyl alcohol fiber is ≥55; more preferably 55-500; further preferably 150-450; and more preferably 300-400.

[0020] The polyvinyl alcohol fiber adopts an aspect ratio within a specific range, which is beneficial to improving the strength of concrete while ensuring that the fiber structure does not form entanglements and affect its dispersion in the slurry.

[0021] Preferably, in the foamed concrete, the mass fraction of the polyvinyl alcohol fiber is 2 to 25 parts; more preferably, it is 3 to 20 parts; and even more preferably, it is 4 to 10 parts.

[0022] Preferably, in the foamed concrete, the mass fraction of water is 150 to 700 parts; more preferably, it is 200 to 650 parts; and even more preferably, it is 300 to 500 parts.

[0023] Preferably, in the foamed concrete, the nano foam is prepared by foaming with a nano foaming agent.

[0024] In some specific embodiments of the present invention, the nano foaming agent is selected from Zhenjiang Yifa Building Materials Nano Foaming Agent NFA-330.

[0025] Preferably, in the foamed concrete, the volume ratio of the nano foam to the cementitious material is (0.5-28):1; more preferably (1-26):1; and even more preferably (2-25):1.

[0026] Preferably, the foamed concrete comprises the following raw materials in proportion by mass: 550 to 1100 parts of cementitious material, 30 to 700 parts of ultrafine filler, 2 to 25 parts of polyvinyl alcohol fiber, and 150 to 700 parts of water; the raw materials also include nano foam, and the volume ratio of the nano foam to the cementitious material is (0.08 to 25):1.

[0027] Further preferably, the foamed concrete comprises the following raw materials in proportion by mass: 600-1000 parts of cementitious material, 60-600 parts of ultrafine filler, 3-20 parts of polyvinyl alcohol fiber, and 200-650 parts of water; the raw materials also include nano foam, and the volume ratio of the nano foam to the cementitious material is (0.1-20):1.

[0028] More preferably, the foamed concrete comprises the following raw materials in proportion by mass: 650 to 800 parts of cementitious material, 150 to 450 parts of ultrafine filler, 4 to 10 parts of polyvinyl alcohol fiber, and 300 to 500 parts of water; the raw materials also include nano foam, and the volume ratio of the nano foam to the cementitious material is (0.2 to 18):1.

[0029] Preferably, in the foamed concrete, the raw materials further include 1 to 500 parts of polyvinyl alcohol; more preferably, the mass fraction of the polyvinyl alcohol is 30 to 400 parts; and even more preferably, it is 100 to 300 parts.

[0030] Adding polyvinyl alcohol can prevent water from being lost to the external environment, and at the same time it can also undergo physical adsorption with the gelling material particles in the slurry. Most importantly, it can provide a stable environment for the nano foam and improve the stability of the nano foam in the slurry.

[0031] Preferably, in the foamed concrete, the degree of polymerization of the polyvinyl alcohol is ≥1700; more preferably, it is 1700-10000; further preferably, it is 1700-5000; non-limiting specific examples are 1800, 2000, 3000 or 4000.

[0032] The use of polyvinyl alcohol with a specific degree of polymerization can ensure its water retention, viscosity-increasing and stabilizing effects while maintaining the fluidity and workability of the slurry.

[0033] Preferably, the foamed concrete comprises the following raw materials in proportion by mass: 500 to 1200 parts of cementitious material, 10 to 800 parts of ultrafine filler, 1 to 30 parts of polyvinyl alcohol fiber, 100 to 800 parts of water, and 1 to 500 parts of polyvinyl alcohol; the raw materials also include nano foam, and the volume ratio of the nano foam to the cementitious material is (0.05 to 30):1.

[0034] Further preferably, the foamed concrete comprises the following raw materials in proportion by mass: 600-1000 parts of cementitious material, 60-600 parts of ultrafine filler, 3-20 parts of polyvinyl alcohol fiber, 200-650 parts of water, and 30-400 parts of polyvinyl alcohol; the raw materials also include nano foam, and the volume ratio of the nano foam to the cementitious material is (0.1-20):1.

[0035] More preferably, the foamed concrete comprises the following raw materials in proportion by mass: 650 to 800 parts of cementitious material, 150 to 450 parts of ultrafine filler, 4 to 10 parts of polyvinyl alcohol fiber, 300 to 500 parts of water, and 100 to 300 parts of polyvinyl alcohol; the raw materials also include nano foam, and the volume ratio of the nano foam to the cementitious material is (0.2 to 18):1.

[0036] Preferably, in the foamed concrete, the raw materials further include 0.1 to 30 parts of a water reducer; more preferably, the mass fraction of the water reducer is 0.5 to 20 parts; and even more preferably, it is 1 to 10 parts.

[0037] Preferably, in the foamed concrete, the water reducer is selected from polycarboxylate water reducer.

[0038] Preferably, the foamed concrete comprises the following raw materials in mass proportions: 500-1200 parts of cementitious material, 10-800 parts of ultrafine filler, 1-30 parts of polyvinyl alcohol fiber, 100-800 parts of water, 1-500 parts of polyvinyl alcohol, and 0.1-30 parts of water reducer; the raw materials also include nano foam, and the volume ratio of the nano foam to the cementitious material is (0.05-30):1;

[0039] Further preferably, the foamed concrete comprises the following raw materials in proportion by mass: 600-1000 parts of cementitious material, 60-600 parts of ultrafine filler, 3-20 parts of polyvinyl alcohol fiber, 200-650 parts of water, 30-400 parts of polyvinyl alcohol, and 0.5-20 parts of water reducer; the raw materials also include nano foam, and the volume ratio of the nano foam to the cementitious material is (0.1-20):1.

[0040] More preferably, the foamed concrete comprises the following raw materials in proportion by weight: 650 to 800 parts of cementitious material, 150 to 450 parts of ultrafine filler, 4 to 10 parts of polyvinyl alcohol fiber, 300 to 500 parts of water, 100 to 300 parts of polyvinyl alcohol, and 1 to 10 parts of water reducer; the raw materials also include nano foam, and the volume ratio of the nano foam to the cementitious material is (0.2 to 18):1.

[0041] The second aspect of the present invention provides a method for preparing the foamed concrete described in the first aspect of the present invention, comprising the following steps: first mixing a cementitious material, an ultrafine filler, polyvinyl alcohol fibers and water, then adding polyvinyl alcohol for a second mixing, then adding nano foam for a third mixing, and obtaining the foamed concrete after grouting molding and curing.

[0042] Preferably, in the preparation method, the first mixing method is selected from stirring; further preferably, the first mixing includes two stages: the rotation speed of the first stage is 50-100 r / min, and the time is 20-40 s; the rotation speed of the second stage is 80-150 r / min, and the time is 30-120 s.

[0043] Preferably, in the preparation method, the second mixing method is selected from stirring; preferably, the rotation speed of the second mixing is 80 to 150 r / min, and the time is 30 to 120 s.

[0044] Preferably, in the preparation method, the third mixing method is selected from stirring; preferably, the rotation speed of the third mixing is 80 to 150 r / min, and the time is 30 to 120 s.

[0045] Preferably, in the preparation method, the material is left to stand for 0 to 8 hours after slip casting, and then autoclaved for 0 to 6 hours.

[0046] Preferably, in the preparation method, the curing time is 10 to 16 hours.

[0047] The third aspect of the present invention provides an application of the foamed concrete described in the first aspect of the present invention in the fields of construction, home furnishing, agriculture or ecological protection.

[0048] Preferably, the present invention provides a door panel comprising the foamed concrete described in the first aspect of the present invention.

[0049] The beneficial effects of the present invention are as follows: by adding nano foam, gelling material, ultrafine filler and polyvinyl alcohol fiber, the present invention effectively accelerates the hydration time of foam concrete, improves the compressive strength and flexural strength of foam concrete, and also increases the closed-cell rate in foam concrete, effectively reduces the water absorption rate and thermal conductivity of foam concrete, and obtains foam concrete with both low bulk density and high strength.

[0050] Specifically, compared with the prior art, the present invention has the following advantages:

[0051] 1. The foamed concrete of the present invention has the characteristics of low bulk density and high strength. 3 The compressive strength is above 0.1MPa; the dry density is 220kg / m 3 The compressive strength is above 0.5MPa; the dry density is 650kg / m 3 When the strength is above 5.5MPa.

[0052] 2. Polyvinyl alcohol fiber (PVA-F) is a synthetic fiber made of polyvinyl alcohol with high polymerization degree as raw material and processed by specific technology. The main characteristics of PVA-F are high strength, high modulus, wear resistance, acid and alkali resistance, weather resistance, excellent, good hydrophilicity, and good compatibility with cement. Due to these characteristics, it can have good interface bonding with cement matrix, and is an ideal material for improving the anti-stripping, tensile resistance, anti-destruction ability and durability of concrete components.

[0053] 3. The present invention can solve the problem that the strength of existing foamed concrete is greatly reduced while reducing the bulk density, thus broadening the application scope of foamed concrete. 3 When the present invention is used, it can replace the existing door panel filling materials, reduce the cost of the door panel, and improve the heat insulation, sound insulation and other properties of the door panel. In addition, since the raw materials of the present invention are mainly inorganic materials, the prepared door panel has a good fireproof effect and can be used as an A1 grade fireproof material.

[0054] 4. The foamed concrete of the present invention is 693kg / m 3 The strength is greater than 5.5MPa, and it can replace building materials such as ALC autoclaved blocks. In addition, because the foamed concrete of the present invention is a silicate system, it has a low water absorption rate and will not shrink in strength. It also adopts physical foaming and can change its shape according to the mold, so it is flexible and convenient to use.

[0055] 5. Compared with ordinary foam concrete, the foam concrete of the present invention has higher specific strength. Under the condition of not collapsing and having a certain strength, its minimum dry density can reach 123kg / m 3 About; at the same dry density, the compressive strength is 150% to 300% of that of ordinary foam concrete; it has a faster hydration time and higher initial strength; it has a higher closed porosity and smaller pore size; it has lower water absorption and thermal conductivity. DETAILED DESCRIPTION

[0056] The content of the present invention is further described in detail below through specific examples. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the principles set forth in the present invention all belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific data exemplified below. The raw materials, reagents or devices used in the following examples and comparative examples, unless otherwise specified, can all be obtained from conventional commercial sources, or can be obtained by existing known methods.

[0057] It should be noted that in the embodiments and comparative examples of the present invention:

[0058] The ultrafine cementitious material is ultrafine silicate cement, D 90 Particle size is 23μm, specific surface area ≥550m 2 / kg;

[0059] The ultrafine filler is produced by Anhui Dongcai Material Technology Co., Ltd. and is mainly composed of ground mineral powder and fly ash. 90 Particle size: 30 μm;

[0060] Polyvinyl alcohol fiber (PVA-F) is a common product on the market with an aspect ratio of 330;

[0061] The nano foaming agent is Zhenjiang Yifa Building Materials Nano Foaming Agent, model number NFA-330;

[0062] Polyvinyl alcohol (PVA) is a common product on the market with a degree of polymerization of 1700;

[0063] The water reducer is polycarboxylic acid water reducer, which is a common product on the market.

[0064] Example 1

[0065] A foamed concrete comprises the following raw materials: 700 g of ultrafine silicate cement, 300 g of ultrafine filler, 5.8 g of PVA-F, 150 g of PVA solution, 4 g of water reducer, 450 mL of water, and 9.03 L of nano foam; the nano foam is obtained by foaming a nano foaming agent (model NFA-330) produced by Zhenjiang Yifa Building Materials.

[0066] The preparation process of the above foamed concrete is as follows:

[0067] S1. Pour ultrafine silicate cement, ultrafine filler and PVA-F into a stirring pot and stir at low speed for 30 seconds, then add water reducer into water and stir, stir at low speed for 10 seconds, then add into the stirring pot, continue stirring at low speed of 50r / min for 30 seconds, then stir at high speed of 150r / min for 1 minute; then adjust the speed and add PVA solution and stir at low speed for 30 seconds, waiting for nano foam to be incorporated;

[0068] S2, using a foaming machine to foam, the nano foam added is in volume;

[0069] S3. Restart the mixer, add the foam to the cement mixture while stirring at a low speed, and stir at a low speed for 1 minute;

[0070] S4. Grouting molding, curing for 8h to 16h under certain conditions, and finally demolding. Before testing the 28-day strength, spray water for curing 2 to 3 times a day under standard curing conditions; after that, spray water every 2 to 3 days.

[0071] Example 2

[0072] A foamed concrete, which is different from Example 1 in that the amount of nano foam used in this example is 6.17 L, and other raw materials and preparation process are the same as those in Example 1.

[0073] Example 3

[0074] A foamed concrete, which is different from Example 1 in that the amount of nano foam used in this example is 4.77 L, and other raw materials and preparation process are the same as those in Example 1.

[0075] Example 4

[0076] A foamed concrete, which is different from Example 1 in that the amount of nano foam used in this example is 3.75 L, and other raw materials and preparation process are the same as those in Example 1.

[0077] Example 5

[0078] A foamed concrete, which is different from Example 1 in that the amount of nano foam used in this example is 2.81 L, and other raw materials and preparation process are the same as those in Example 1.

[0079] Example 6

[0080] A foamed concrete, which is different from Example 1 in that the ultrafine silicate cement is replaced with 525 silicate cement (D 90 The particle size is 70 μm), and the amount of nano foam used is 1.06 L. Other raw materials and preparation process are the same as those in Example 1.

[0081] Table 1 shows the raw material compositions and wet bulk densities of the foamed concretes of Examples 1 to 6.

[0082] Table 1 Raw material composition and wet bulk density of foamed concrete of Examples 1 to 6

[0083]

[0084] Comparative Example 1

[0085] A foamed concrete, which is different from Example 1 in that the ultrafine silicate cement is replaced with 525 silicate cement (D 90 The particle size is 70 μm) and the dosage is modified to 1000 g, the nano foam is replaced by commercially available general foam (purchased from Raymer Chemical: concentrated high-efficiency cement foaming agent, compared with the nano foam, the commercially available general foam has worse stability in cement, higher defoaming rate and larger pore size), no PVA solution and ultrafine filler are added, and other raw materials and preparation process are the same as those in Example 1.

[0086] Comparative Example 2

[0087] A foamed concrete, which is different from Comparative Example 1 in that the amount of nano foam used in this example is 6.17 L, and other raw materials and preparation process are the same as those of Comparative Example 1.

[0088] Comparative Example 3

[0089] A foamed concrete, which is different from Comparative Example 1 in that the amount of nano foam used in this example is 4.77 L, and other raw materials and preparation process are the same as those of Comparative Example 1.

[0090] Comparative Example 4

[0091] A foamed concrete, which is different from Comparative Example 1 in that the amount of nano foam used in this example is 3.75 L, the amount of water used is 400 mL, and other raw materials and preparation process are the same as those of Comparative Example 1.

[0092] Comparative Example 5

[0093] A foamed concrete, which is different from Comparative Example 1 in that the amount of nano foam used in this example is 2.81 L, the amount of water used is 400 mL, and other raw materials and preparation process are the same as those of Comparative Example 1.

[0094] Comparative Example 6

[0095] A foamed concrete, which is different from Comparative Example 1 in that the amount of nano foam used in this example is 1.06 L, the amount of water used is 350 mL, and other raw materials and preparation process are the same as those of Comparative Example 1.

[0096] The raw material compositions and wet bulk densities of the foamed concretes of Comparative Examples 1 to 6 are shown in Table 2.

[0097] Table 2 Raw material composition and wet bulk density of foamed concrete of comparative examples 1 to 6

[0098]

[0099] Performance Testing

[0100] After the foamed concrete of Examples 1 to 6 and Comparative Examples 1 to 6 was cured for 28 days, the 28-day compressive strength was tested according to JG / T 266-2011. The results are shown in Table 3.

[0101] Table 3 Dry bulk density and 28-day compressive strength of foamed concrete of Examples 1 to 6 and Comparative Examples 1 to 6

[0102]

[0103]

[0104] As can be seen from Table 3, compared with Examples 1 to 7, the foamed concrete prepared in Examples 1 to 7 of the present invention has a lower density and a higher strength at the same density. In particular, since no PVA solution is added in Example 7, the foam environment is not as stable as in Example 1, the pore diameter of the foam increases, and the strength decreases, but it still has a lower bulk density and a higher strength as a whole.

[0105] The foamed concrete of Examples 1 to 7 of the present invention has the characteristics of low bulk density and high strength. 3 The compressive strength is above 0.1MPa; the dry density is 220kg / m 3 The compressive strength is above 0.5MPa; the dry density is 650kg / m 3 When the strength is above 5.5MPa.

[0106] The polyvinyl alcohol fiber (PVA-F) used in Examples 1 to 7 of the present invention is a synthetic fiber made of polyvinyl alcohol with a high degree of polymerization and processed using a specific technology. The main characteristics of PVA-F are high strength, high modulus, wear resistance, acid and alkali resistance, weather resistance, excellent and good hydrophilicity, and good compatibility with cement. Due to these characteristics, it can have a good interface bonding force with the cement matrix, and is an ideal material for improving the anti-stripping, tensile strength, anti-destruction ability and durability of concrete components.

[0107] The foamed concrete of Examples 1 to 7 of the present invention can solve the problem that the strength of the existing foamed concrete is greatly reduced while the bulk density is reduced, thereby broadening the application scope of the foamed concrete. 3 When the present invention is used, it can replace the existing door panel filling materials, reduce the cost of the door panel, and improve the heat insulation, sound insulation and other properties of the door panel. In addition, since the raw materials of the present invention are mainly inorganic materials, the prepared door panel has a good fireproof effect and can be used as an A1 grade fireproof material.

[0108] The foamed concrete of Examples 1 to 7 of the present invention is heated to 693 kg / m 3 The strength is greater than 5.5MPa, and it can replace building materials such as ALC autoclaved blocks. In addition, because the foamed concrete of the present invention is a silicate system, it has a low water absorption rate and will not shrink in strength. It also adopts physical foaming and can change its shape according to the mold, so it is flexible and convenient to use.

[0109] Compared with ordinary foamed concrete, the foamed concrete in Examples 1 to 7 of the present invention has a higher specific strength. Under the condition of not collapsing and having a certain strength, its dry density can reach a minimum of 123 kg / m 3About; at the same dry density, the compressive strength is 150% to 300% of that of ordinary foam concrete; it has a faster hydration time and higher initial strength; it has a higher closed porosity and smaller pore size; it has lower water absorption and thermal conductivity.

[0110] In summary, the present invention effectively accelerates the hydration time of foamed concrete, improves the compressive and flexural strengths of foamed concrete, and also increases the closed-cell rate in foamed concrete, effectively reduces the water absorption rate and thermal conductivity of foamed concrete, thereby obtaining foamed concrete with both low bulk density and high strength by adding nano foam, gelling material, ultrafine filler and polyvinyl alcohol fiber.

Claims

1. A foamed concrete, characterized in that: The invention comprises the following raw materials in parts by weight: 500 to 1200 parts of gelling material, 10 to 800 parts of ultrafine filler, 1 to 30 parts of polyvinyl alcohol fiber, and 100 to 800 parts of water; the raw materials also include nano foam, and the volume ratio of the nano foam to the gelling material is (0.05 to 30): 1; the particle size range of the ultrafine filler is 1 to 50 μm.

2. The foamed concrete according to claim 1, characterized in that The particle size of the gelling material is in the range of 1 to 40 μm; and / or the specific surface area of ​​the gelling material is ≥550 m 2 / kg.

3. The foamed concrete according to claim 1, characterized in that The cementitious material is selected from cement; preferably, the cement is selected from Portland cement; And / or, the ultrafine filler includes mineral powder and / or fly ash.

4. The foamed concrete according to claim 1, characterized in that The aspect ratio of the polyvinyl alcohol fiber is ≥55.

5. The foamed concrete according to claim 1, characterized in that The nano foam is prepared by foaming a nano foaming agent.

6. The foamed concrete according to claim 1, characterized in that The raw materials also include 1 to 500 parts of polyvinyl alcohol; preferably, the degree of polymerization of the polyvinyl alcohol is ≥1700.

7. The foamed concrete according to claim 1, characterized in that The raw materials also include 0.1 to 30 parts of a water reducer; preferably, the water reducer is selected from polycarboxylate water reducer.

8. A method for preparing foamed concrete according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: first mixing gelling material, ultrafine filler, polyvinyl alcohol fiber and water, then adding polyvinyl alcohol for second mixing, then adding nano foam for third mixing, and obtaining the foam concrete after grouting molding and curing.

9. Use of the foamed concrete according to any one of claims 1 to 7 in the fields of construction, home furnishing, agriculture or ecological protection.

10. A door panel, characterized in that: The foamed concrete comprises the foamed concrete according to any one of claims 1 to 7.

Citation Information

Patent Citations

  • Super-light foam concrete and preparation method thereof

    CN107324735A

  • Lightweight high-strength cement-based foam thermal insulation material and preparation method thereof

    CN111689790A

  • Cast-in-place nano foam concrete as well as preparation method and application thereof