Blocking mortar for rockfill self-compacting concrete formwork

By using stone-stuffed concrete formwork in the pumping pipeline to seal the mortar, combining starch-polyacrylate composite and acrylate-acrylamide copolymer, the problem of poor airtightness during pumping of ultra-long pipelines is solved, and the problem of poor airtightness during pumping is improved. The density and construction efficiency of the pipeline are ensured, and the quality of the concrete is ensured.

CN118978369APending Publication Date: 2024-11-19CHONGQING HUAXI YITONG CONSTR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411069107.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

During the process of pumping concrete in ultra-long pipelines, poor air tightness causes air to enter the pipeline system, affecting construction efficiency and concrete quality, especially when high-strength concrete is pumped, resulting in bubbles and pipe blockage problems.

Method used

A stone-stuffed concrete formwork is used to seal the mortar, including cement, stone pile, natural sand, expansion agent and thickener. The mortar is enhanced by starch-polyacrylate composite and acrylate-acrylamide copolymer and other additives. The compactness, adhesion and crack resistance ensure the airtightness at the pipe joints.

Benefits of technology

It significantly improves the air tightness of the pipeline, prevents air from entering, reduces pumping resistance and energy consumption, improves construction efficiency and concrete quality, and enhances the adhesion and durability of the mortar.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the field of pump concrete, and particularly discloses blocking mortar for a rock-fill self-compacting concrete formwork. The rockfill self-compacting concrete template plugging mortar is prepared from the following components in parts by weight: 400 to 500 parts of cement, 800 to 900 parts of rockfill, 700 to 900 parts of natural sand, 150 to 250 parts of water, 20 to 40 parts of a water reducing agent, 50 to 100 parts of an expanding agent and 1 to 10 parts of a thickening agent. The rockfill self-compacting concrete formwork plugging mortar has the advantage that the air tightness of a pumping pipeline is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of pumped concrete, and more specifically, to a rockfill self-compacting concrete formwork sealing mortar. Background Art

[0002] With the acceleration of urbanization and the continuous advancement of construction technology, high-rise buildings are rising rapidly around the world. High-rise buildings can not only effectively utilize limited urban land resources, but also play an important role in improving the city's image and optimizing urban functions. In the construction process of these high-rise buildings, concrete pumping technology, as one of the key construction technologies, is particularly important. High-rise pumping concrete technology originated in the mid-20th century. With the increase in demand for high-rise buildings and the advancement of concrete construction technology, pumping technology has gradually been widely used. Pumping concrete technology mainly uses concrete pumps to transport the mixed concrete to the designated location of the construction site through pipelines. The application of this technology has greatly improved construction efficiency and concrete pouring quality.

[0003] However, with the increasing number of super-high-rise buildings, the problem of poor air tightness has gradually emerged in the process of pumping concrete through super-long pipelines. In the process of super-long pipeline pumping, there are many pipeline connection points. If the connection is not tight, it is easy for air to enter the pipeline system, resulting in poor air tightness. Pipes that have been used for a long time are prone to wear and tear, especially when pumping high-strength concrete. Worn pipes are prone to cracks, allowing air to enter. Poor air tightness can cause problems such as bubbles and pipe blockage during concrete pumping, affecting construction efficiency and concrete quality. Summary of the invention

[0004] In order to improve the air tightness of a pumping pipeline, the present application provides a rockfill self-compacting concrete formwork plugging mortar.

[0005] The present application provides a rockfill self-compacting concrete formwork plugging mortar adopts the following technical solution: A self-compacting rockfill concrete formwork sealing mortar comprises, by weight, 400-500 parts of cement, 800-900 parts of rockfill, 700-900 parts of natural sand, 150-250 parts of water, 20-40 parts of water reducing agent, 50-100 parts of expansion agent and 1-10 parts of thickener.

[0006] By adopting the above technical solution, cement is used as the main cementitious material to provide the basic strength and bonding performance of the mortar. The rockfill acts as an aggregate to improve the density of the mortar, thereby improving the air tightness at the pipe joints by filling the gaps. Natural sand is used in combination with rockfill to fill the gaps in the concrete, enhance the density, further improve the density of the mortar, and prevent air from entering the pipeline system. The expansion agent produces micro-expansion during the hardening process, fills the tiny gaps in the pipeline, prevents shrinkage and cracking, ensures the close connection between the mortar and the pipeline, and improves the air tightness. The thickener enhances the viscosity of the mortar, prevents stratification and segregation, ensures the uniformity and stability of the mortar during the construction process, and further improves the air tightness.

[0007] Optionally, 10-30 parts of starch-polyacrylic acid salt compound is also included, and the preparation method of the starch-polyacrylic acid salt compound is as follows: Dissolve 60-80 parts of corn starch by weight in 120 parts of water, stir and heat to 80-90°C to completely gelatinize and form starch slurry; Dissolve 40-60 parts of acrylic acid in 120 parts of water, adjust the pH value to 7-8, add 1-5 parts of azobisisobutyronitrile and 10-20 parts of polyphosphoric acid to the acrylic acid solution, stir well, add the acrylic acid solution dropwise to the starch slurry, stir well, maintain the reaction temperature at 60-70°C, and react for about 2-3 hours; After the reaction is completed, the mixture is cooled to room temperature, the product is filtered, vacuum dried to constant weight, and crushed to 0.1-0.5 mm to obtain a starch-polyacrylic acid salt complex.

[0008] By adopting the above technical scheme, the polyacrylic acid salt in the starch-polyacrylic acid salt complex has excellent water retention and thickening properties, can form a stable colloidal structure in the mortar, effectively prevent the segregation and stratification of the mortar during the pumping process, and improve the uniformity and stability of the mortar. At the same time, this compound can also react well with cementitious materials such as cement to further enhance the adhesion and durability of the mortar. After gelatinization and polymerization, the starch in the starch-polyacrylic acid salt complex can form a mesh structure with a certain elasticity, which can effectively prevent the mortar from cracking during the hardening process and improve the crack resistance of the mortar. At the same time, the compound can also fill the tiny gaps in the mortar, reduce the air entering the pipeline system, and further improve the air tightness of the mortar. The addition of the starch-polyacrylic acid salt complex further optimizes the fluidity of the mortar, enables it to flow more smoothly in the pipeline, reduces the resistance and energy consumption during the pumping process, and improves the construction efficiency.

[0009] Optionally, it also includes 5-15 parts of acrylate-acrylamide copolymer, and the preparation method of the acrylate-acrylamide copolymer is as follows: Acrylate, acrylamide and deionized water are mixed and stirred at a mass ratio of (1-3):1:3 to obtain a mixed solution; 1-10% by weight of ammonium persulfate and 20-40% by weight of N,N'-methylenebisacrylamide are added to the mixed solution, stirred evenly, the temperature is controlled at 40-60°C, and stirred for 3-4 hours; After the reaction is completed, the product is cooled to room temperature, vacuum dried to constant weight, and the dried product is crushed to 0.1-0.5 mm to obtain an acrylate-acrylamide copolymer.

[0010] By adopting the above technical solution, the acrylate-acrylamide copolymer has excellent adhesion and cohesion, and can react well with cementitious materials such as cement to form stronger chemical bonds. This can not only enhance the adhesion between the mortar and the pipe wall, formwork and other substrates, but also enter the pipe to fill the gap and improve the air tightness in the pipe during the delivery process. The acrylate-acrylamide copolymer has a certain lubricating effect, which can reduce the friction resistance of the mortar and improve its fluidity and pumpability. This allows the mortar to flow more smoothly in the pipe, reduce the resistance and energy consumption during the pumping process, and improve construction efficiency.

[0011] Optionally, the thickener is one or more of nano silicon powder and carboxymethyl cellulose.

[0012] By adopting the above technical solution, nano silicon powder has a very small particle size and a high specific surface area, which can fill the tiny gaps in the mortar, improve the density of the mortar, and enable the mortar to better enter the gaps in the pumping pipeline and bond and seal. At the same time, the addition of nano silicon powder can optimize the rheological properties of the mortar, making it flow more smoothly in the pipeline and reducing the resistance and energy consumption during the pumping process.

[0013] Optionally, the rockfill is made of crushed stone with a particle size of 5-10 mm, and the natural sand is made of river sand with a particle size of 0.5-2 mm.

[0014] By adopting the above technical solution, the mortar contains 800-900 parts of rockfill, which can be used as aggregate to effectively fill the gaps in the pipe. In particular, when crushed stone with a particle size of 5-10 mm is selected as the rockfill, its moderate particle size can better adapt to the complex spatial structure inside the pipe and achieve a tighter filling. Due to the tight filling of the rockfill and self-compacting concrete, the density of the mortar is greatly improved, which effectively prevents the infiltration of air and improves the air tightness of the pipe. The rockfill and self-compacting concrete in the mortar work together to enhance the crack resistance of the mortar and reduce the problem of air infiltration caused by cracks.

[0015] Optionally, the water reducer is a polycarboxylate water reducer or a naphthalene water reducer.

[0016] By adopting the above technical solution, the water reducing agent used in this application has excellent water reducing performance, does not have obvious segregation and water seepage, is easy to stir and construct, and is extremely beneficial for long-distance transportation and pumping construction.

[0017] Optionally, the expansion agent is one of calcium sulphoaluminate and magnesium oxysulfate.

[0018] By adopting the above technical solution, the calcium sulfoaluminate expansion agent can produce a moderate volume expansion after reacting with water in concrete. This expansion can effectively fill the gaps in the pumping pipeline and increase the density of the concrete. Due to the expansion effect of the calcium sulfoaluminate expansion agent, the concrete can better fill the gaps during the flow process in the pipeline, reduce the porosity in the concrete, and thus improve the density of the concrete. As the density of the concrete increases, its impermeability will also be enhanced accordingly. This helps to prevent the penetration of moisture and harmful substances and further improve the air tightness of the pipeline. The magnesium oxysulfate expansion agent also has expansion properties, can fill the gaps in the pipeline, improve the density of the concrete, and can also improve the microstructure of the system, fill the gaps and pores of the system, and improve the volume stability, which also helps to improve the air tightness of the pipeline.

[0019] In a second aspect, the present application provides a method for preparing a rockfill self-compacting concrete formwork plugging mortar, which adopts the following technical solution: A method for preparing a rockfill self-compacting concrete formwork plugging mortar comprises the following steps: First add cement, rockfill, and natural sand into the mixer and stir at low speed for 2-5 minutes to make them evenly mixed; Gradually add water and continue stirring until mixed evenly. While continuing to stir, add water reducer, expander and thickener for about 5-10 minutes until the slurry is uniform and free of lumps.

[0020] Optionally, after adding the water reducing agent, the swelling agent and the thickening agent, a starch-polyacrylic acid salt complex and an acrylate-acrylamide copolymer need to be added.

[0021] By adopting the above technical solution, cement, rockfill and natural sand are first added to the mixer, and these materials are initially evenly mixed by stirring at a low speed for 2-5 minutes, and then water is gradually added and stirred until they are evenly mixed. This step ensures that water is fully in contact with dry materials such as cement, promotes hydration, and provides a basis for the strength development of the mortar. The addition of water reducer significantly improves the fluidity of the mortar, making it easier to pump and fill; the addition of expansion agent helps to fill the tiny gaps in the pipe and improve the density; the addition of thickener helps to improve the viscosity of the mortar and prevent segregation and bleeding. The optional addition of starch-polyacrylic acid salt complex and acrylate-acrylamide copolymer will further enhance the performance of the mortar. Starch-polyacrylic acid salt complex can improve the adhesion and water retention of the mortar, while acrylate-acrylamide copolymer can improve the durability and crack resistance of the mortar.

[0022] In summary, this application has the following beneficial effects: 1. Since this application uses cement as the basic cementitious material to provide key strength and bonding properties for the mortar, and the rockfill and natural sand are used as aggregates to fill the voids in the concrete, significantly improving the density of the mortar, thereby effectively preventing air infiltration and improving the air tightness of the pipe joints. In addition, the micro-expansion of the expansion agent during the hardening process further fills the tiny voids, avoids shrinkage and cracking, and ensures that the mortar is tightly combined with the pipe; the thickener enhances the viscosity of the mortar, maintains its uniformity and stability, and ultimately comprehensively improves the air tightness of the pipeline system.

[0023] 2. In this application, starch-polyacrylic acid salt composite is preferably used. The composite reacts well with cement and other cementitious materials to enhance the adhesion and durability of the mortar. The elastic network structure formed by the starch treatment effectively prevents the generation of cracks during the hardening process of the mortar and improves the crack resistance. In addition, the composite can fill the tiny gaps in the mortar, enhance the air tightness, optimize the fluidity of the mortar, make the mortar easier to flow in the pipeline, reduce the construction difficulty, and improve the construction efficiency.

[0024] 3. In the present application, the introduction of acrylate-acrylamide copolymer is preferably used to significantly enhance the multiple properties of the mortar. Its excellent adhesion and cohesion not only strengthen the adhesion between the mortar and the pipe wall, formwork and other substrates, but also improve the internal density and integrity of the mortar, effectively reducing cracks and gaps. At the same time, the lubricating effect of the copolymer improves the fluidity and pumpability of the mortar, making it flow more smoothly in the pipeline, reducing construction resistance and energy consumption, and improving construction efficiency. In addition, the acrylate-acrylamide copolymer also gives the mortar excellent impermeability and air tightness, effectively preventing the penetration of moisture and air, and further ensuring the quality and durability of the concrete. DETAILED DESCRIPTION

[0025] The present application is further described in detail below in conjunction with the examples. It is particularly noted that if no specific conditions are specified in the following examples, the experiments are carried out according to conventional conditions or the conditions recommended by the manufacturer. Unless otherwise specified, the raw materials used in the following examples can be obtained from common commercial sources.

[0026] Preparation example of starch-polyacrylic acid salt complex Preparation Example 1 Preparation of starch-polyacrylic acid salt complex: Add 70 kg corn starch into 120 kg water and stir until completely dissolved. Then heat the reactor containing the corn starch solution to 85°C and continue stirring at 60 r / min with a stirrer to completely gelatinize and form a starch slurry. Dissolve 50kg of acrylic acid in 120kg of water, adjust the pH value to 7-8 with 10% sodium hydroxide solution, add 3kg of azobisisobutyronitrile and 15kg of polyphosphoric acid to the acrylic acid solution, stir well, add the acrylic acid solution to the starch slurry, add the starch slurry in 30 minutes, stir well, maintain the reaction temperature at 65°C, and react for about 3 hours; After the reaction is completed, the mixture is cooled to room temperature, the reaction product is centrifuged and filtered, vacuum dried at 40°C to constant weight, and crushed to 0.1-0.5 mm to obtain a starch-polyacrylic acid salt complex.

[0027] Preparation Example 2 Preparation of starch-polyacrylic acid salt complex: The difference from Preparation Example 1 is that no sodium hydroxide solution is used to adjust the pH.

[0028] Preparation Example 3 Preparation of starch-polyacrylic acid salt composite: The difference from Preparation Example 1 is that azobisisobutyronitrile is not added.

[0029] Preparation Example of Acrylate-Acrylamide Copolymer Preparation Example 4 Preparation of Acrylate-Acrylamide Copolymer: 20 kg of acrylate, 10 kg of acrylamide and 30 kg of deionized water were added into a reaction kettle and mixed and stirred evenly by a stirrer to obtain a mixed solution; Add 1.5 kg of ammonium persulfate and 9 kg of N,N'-methylenebisacrylamide to the mixed solution, stir evenly, control the temperature at 50°C, and stir for 3 hours; After the reaction is completed, the product is cooled to room temperature, vacuum dried to constant weight, and the dried product is crushed to 0.1-0.5 mm to obtain an acrylate-acrylamide copolymer.

[0030] Preparation Example 5 Preparation of Acrylate-Acrylamide Copolymer: The difference from Preparation Example 4 is that no ammonium persulfate is added.

[0031] Preparation Example 6 Preparation of acrylate-acrylamide copolymer: The difference from Preparation Example 4 is that 5 kg of acrylate, 10 kg of acrylamide and 30 kg of deionized water are added into the reaction kettle and mixed. Example

[0032] Example 1 Preparation of a rockfill self-compacting concrete formwork plugging mortar: First add 45kg 42.5R Portland cement, 85kg crushed stone with a particle size of 5-10mm, and 80kg river sand with a particle size of 0.5-2mm into the mixer, and stir at low speed for 5 minutes to mix them evenly; Gradually add 20 kg of water and continue stirring until it is evenly mixed. While continuing to stir, add 3 kg of water reducer, 8 kg of expansion agent and 0.5 kg of thickener. Stir for 10 minutes until the slurry is uniform and free of lumps.

[0033] Among them, the water reducer is BF-01 polycarboxylic acid water reducer produced by Shandong Bofei Cement Technology Service Co., Ltd., the expansion agent is calcium sulfoaluminate, and the thickener is nano silicon powder.

[0034] Example 2 Preparation of a rockfill self-compacting concrete formwork plugging mortar: First add 45kg 42.5R Portland cement, 85kg crushed stone with a particle size of 5-10mm, and 80kg river sand with a particle size of 0.5-2mm into the mixer, and stir at low speed for 5 minutes to mix them evenly; Gradually add 20 kg of water and continue stirring until it is evenly mixed. While continuing to stir, add 3 kg of water reducer, 8 kg of expander, 0.5 kg of thickener, and 2 kg of starch-polyacrylic acid salt complex. Stir for 10 minutes until the slurry is uniform and free of lumps.

[0035] Among them, the water reducer is BF-01 water reducer produced by Shandong Bofei Cement Technology Service Co., Ltd., the expansion agent is calcium sulfoaluminate, the thickener is nano silicon powder, and the starch-polyacrylic acid salt complex is prepared by Preparation Example 1.

[0036] Example 3 Preparation of a rockfill self-compacting concrete formwork plugging mortar: First add 45kg 42.5R Portland cement, 85kg crushed stone with a particle size of 5-10mm, and 80kg river sand with a particle size of 0.5-2mm into the mixer, and stir at low speed for 5 minutes to mix them evenly; Gradually add 20 kg of water and continue stirring until mixed evenly. While continuing to stir, add 3 kg of water reducer, 8 kg of expander, 0.5 kg of thickener, 2 kg of starch-polyacrylic acid salt complex, and 1 kg of acrylate-acrylamide copolymer. Stir for 10 minutes until the slurry is uniform and free of lumps.

[0037] Among them, the water reducer is BF-01 water reducer produced by Shandong Bofei Cement Technology Service Co., Ltd., the expansion agent is calcium sulfoaluminate, the thickener is nano silicon powder, the starch-polyacrylate complex is prepared by Preparation Example 1, and the acrylate-acrylamide copolymer is prepared by Preparation Example 4.

[0038] Example 4 Preparation of a rockfill self-compacting concrete formwork plugging mortar: The difference from Example 3 is that the water reducer is the Wanshan brand naphthalene-based water reducer produced by Jinan Runfeng Chemical Co., Ltd.

[0039] Example 5 Preparation of a rockfill self-compacting concrete formwork sealing mortar: The difference from Example 3 is that the expansion agent is magnesium oxysulfate.

[0040] Example 6 Preparation of a rockfill self-compacting concrete formwork sealing mortar: The difference from Example 3 is that carboxymethyl cellulose is used as the thickener.

[0041] Comparative Example Comparative Example 1 Preparation of a rockfill self-compacting concrete formwork sealing mortar: The difference from Example 3 is that the starch-polyacrylic acid salt composite is prepared by Preparation Example 2.

[0042] Comparative Example 2 Preparation of a rockfill self-compacting concrete formwork sealing mortar: The difference from Example 3 is that the starch-polyacrylic acid salt composite is prepared by Preparation Example 3.

[0043] Comparative Example 3 Preparation of a rockfill self-compacting concrete formwork sealing mortar: The difference from Example 3 is that the acrylate-acrylamide copolymer is prepared by Preparation Example 5.

[0044] Comparative Example 4 Preparation of a rockfill self-compacting concrete formwork sealing mortar: The difference from Example 3 is that the acrylate-acrylamide copolymer is prepared by Preparation Example 6.

[0045] Performance testing Detection Methods Select 10 sections of 10m long pumping pipelines and manually process them to achieve air tightness with a leakage rate of 1±0.1m 3 / min, and then pump the plugging mortar prepared in the embodiment and the comparative example once respectively. After the pumping is completed, the pumping pipeline is placed under natural conditions for 48 hours, and then the pipeline is connected to the standard container, and the joint is sealed with sealant. A pressure of 5 times the atmospheric pressure is applied to the standard container to allow gas to enter the pipeline. After the pressure stabilizes, a flow meter is used to measure the amount of gas escaping per unit time.

[0046] Table 1 Test data Example 1 Example 2 Example 3 Example 4 Example 5 Leakage 0.35 0.23 0.12 0.14 0.13 Example 6 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Leakage 0.15 0.20 0.22 0.19 0.21 It can be seen from Example 3 and Comparative Examples 1-2 and Table 1 that if the pH value is not adjusted during the preparation of the starch-polyacrylate composite, the purity of the composition will be affected. This is because acrylic acid will self-polymerize under acidic conditions, resulting in reduced purity of the product, affecting its ability to seal and fill the pipe after adding mortar. Azobisisobutyronitrile is used as an initiator, and if it is not added, the degree of polymerization will be reduced. Preparation Example 1 in this application is the best choice.

[0047] It can be seen from Example 3 and Comparative Examples 3-4 and Table 1 that failure to add ammonium sulfate will reduce the purity of the product, thereby causing the effect of the mortar to deteriorate. Preparation Example 4 in this application is the best choice.

[0048] It can be seen from Examples 1-3 and Table 1 that the starch in the starch-polyacrylic acid salt composite can form a network structure with a certain elasticity after gelatinization and polymerization reaction, which can fill the tiny gaps in the mortar, reduce the air entering the pipeline system, and further improve the air tightness of the mortar. The acrylate-acrylamide copolymer has excellent adhesion and cohesion, can react well with cementitious materials such as cement to form a stronger chemical bond, can enter the pipeline to fill the gap, and improve the air tightness of the pipeline during the delivery process.

[0049] It can be seen from Examples 3-6 and Table 1 that when nano-silicon powder is used as the thickener, polycarboxylic acid water-reducing agent is used as the water-reducing agent, and calcium sulphoaluminate is used as the swelling agent, the mortar can better fill the gaps and improve the air tightness.

[0050] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed. However, as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.

Claims

1. A self-compacting rockfill concrete formwork sealing mortar, characterized in that: The invention comprises, by weight, 400-500 parts of cement, 800-900 parts of rockfill, 700-900 parts of natural sand, 150-250 parts of water, 20-40 parts of water reducer, 50-100 parts of expansion agent and 1-10 parts of thickener.

2. The self-compacting rockfill concrete formwork sealing mortar according to claim 1, characterized in that: The invention also includes 10-30 parts of a starch-polyacrylic acid salt complex, wherein the starch-polyacrylic acid salt complex is prepared by: Dissolve 60-80 parts of corn starch in 120 parts of water, stirring and heating to 80-90°C to completely gelatinize and form a starch slurry; Dissolve 40-60 parts of acrylic acid in 120 parts of water, adjust the pH to 7-8, add 1-5 parts of azobisisobutyronitrile and 10-20 parts of polyphosphoric acid to the acrylic acid solution, stir thoroughly, add the acrylic acid solution dropwise to the starch slurry, stir well, maintain the reaction temperature at 60-70°C, and react for about 2-3 hours; After the reaction is completed, the mixture is cooled to room temperature, the product is filtered, vacuum dried to constant weight, and crushed to 0.1-0.5 mm to obtain a starch-polyacrylic acid salt complex.

3. The self-compacting rockfill concrete formwork sealing mortar according to claim 1, characterized in that: It also includes 5-15 parts of acrylate-acrylamide copolymer, and the preparation method of the acrylate-acrylamide copolymer is as follows: Acrylate, acrylamide and deionized water were mixed in a mass ratio of (1-3):1:3 and stirred to obtain a mixed solution; Add 1-10% of the solute weight of ammonium persulfate and 20-40% of the solute weight of N,N'-methylenebisacrylamide to the mixed solution, stir evenly, control the temperature at 40-60°C, and stir for 3-4 hours; After the reaction is completed, the product is cooled to room temperature and vacuum dried to constant weight. The dried product is crushed to 0.1-0.5 mm to obtain an acrylate-acrylamide copolymer.

4. The self-compacting rockfill concrete formwork sealing mortar according to claim 1, characterized in that: The thickener is selected from one or more of nano silicon powder and carboxymethyl cellulose.

5. The self-compacting rockfill concrete formwork sealing mortar according to claim 1, characterized in that: The rockfill is made of crushed stone with a particle size of 5-10 mm, and the natural sand is made of river sand with a particle size of 0.5-2 mm.

6. The self-compacting rockfill concrete formwork sealing mortar according to claim 1, characterized in that: The water reducer is selected from one of polycarboxylic acid water reducer and naphthalene water reducer.

7. The self-compacting rockfill concrete formwork sealing mortar according to claim 1, characterized in that: The expansion agent is selected from calcium sulfoaluminate and magnesium oxysulfate.

8. A method for preparing the self-compacting rockfill concrete formwork sealing mortar according to any one of claims 1 to 7, characterized in that: The following steps are involved: First add cement, rockfill, and natural sand into the mixer and stir at low speed for 2-5 minutes to mix them evenly; Gradually add water and continue stirring until the mixture is evenly mixed. While continuing to stir, add the water reducer, expander and thickener and stir for 5-10 minutes until the slurry is uniform and there are no lumps.

9. The method for preparing the rockfill self-compacting concrete formwork sealing mortar according to claim 8, characterized in that: After adding the water reducing agent, the swelling agent and the thickening agent, the starch-polyacrylic acid salt complex and the acrylate-acrylamide copolymer need to be added.