Seawater-corrosion-resistant offshore wind power grouting material and preparation method thereof
Through the combination of high-iron phase silicate cement, sulfoaluminate cement and doped barium salt silica aerogel, the lack of fluidity, strength and durability of offshore wind grouting materials is solved, and efficient Preparation of offshore wind power grouting materials to meet the needs of offshore wind power infrastructure.
Patent Information
- Application Number
- CN202410946644.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-19
AI Technical Summary
The existing grouting materials cannot meet the needs of high liquidity, high early strength, minor expansion, no contraction in the later stage and resistance to seawater erosion in offshore wind power applications, and are not very durable.
The raw materials such as high-iron phase silicate cement, sulfur aluminate cement, seawater corrosion resistance and barium salt-doped silica aerogels are used to form high fluidity, early strength and Offshore wind grouting material with excellent durability.
Offshore wind power grouting materials are achieved with high initial flow, high early compressive strength, minor expansion and no shrinkage, excellent seawater erosion resistance and good durability, and are suitable for infrastructure construction of the marine environment.
Smart Images

Figure BDA0004945849960000031 
Figure BDA0004945849960000041 
Figure BDA0004945849960000042
Abstract
Description
Technical Field
[0001] The invention belongs to the field of grouting materials, and in particular relates to an offshore wind power grouting material resistant to seawater erosion and a preparation method thereof. Background Art
[0002] Offshore wind power grouting materials are mainly used in offshore wind power construction, including grouting of the upper module of the offshore booster station, grouting of the foundation of the offshore booster station jacket, grouting of the transition section of the single pile, underwater grouting of the foundation of the wind turbine jacket, and structural grouting of the connector of the wind turbine foundation anti-collision facility. The wind power grouting connection section connects the upper structure and the pile foundation into a whole and plays a transitional role. It is a key link in the entire foundation structure. The construction of the foundation structure of offshore wind turbines is far more complicated than that of onshore ones, with high technical difficulty and a cost as high as 15%-25% of the total cost. The particularity of offshore wind power grouting is that the material is required to have high flow viscosity and high stability in the pumping liquid phase, and the grouting material is required to have ultra-high strength, micro-expansion and high durability after hardening.
[0003] Compared with the stringent technical requirements of wind power grouting, the current high-end domestic grouting products can generally solve special needs for a single indicator. For example, the special mortar for high-speed rail supports mainly solves high fluidity and high hourly strength. The grouting materials used for prefabricated component node connections in residential industrialization projects require high fluidity, high filling properties and high strength. The grouting materials for holes in prestressed structures mainly solve the problem of grouting of holes, etc. However, the strength and durability of these grouting materials are not high and cannot meet the grouting requirements of offshore wind turbines.
[0004] Therefore, there is an urgent need for a micro-expansion grouting material for offshore wind turbine grouting, which has high flow viscosity and high stability in the early grouting stage, and has ultra-high strength, micro-expansion and high durability after the grouting hardens. Summary of the invention
[0005] Purpose of the invention: The technical problem to be solved by the present invention is to provide a grouting material suitable for offshore wind power infrastructure construction, which has not only high fluidity, high early strength, slight expansion, no shrinkage in the later period, but also excellent resistance to seawater erosion and excellent water tightness, and a preparation method thereof.
[0006] Technical solution: The offshore wind power grouting material resistant to seawater erosion of the present invention comprises the following raw materials by weight: 40-45 parts of high-iron phase silicate cement, 5-10 parts of sulphoaluminate cement, 5-10 parts of anti-seawater erosion agent, 5-10 parts of expansion component, 34-42 parts of fine aggregate, 0.5-1 part of silicon dioxide aerogel doped with barium salt, and 0.4-0.5 part of water reducer.
[0007] The invention is based on the basic components of high-iron phase silicate cement, sulphoaluminate cement, fine aggregate, expansion component and water reducer, and compounded with seawater erosion resistance agent and silicon dioxide aerogel doped with barium salt to form an offshore wind power grouting material suitable for marine environment. The application of high iron phase silicate cement and sulphoaluminate cement in offshore wind power grouting materials not only improves the wind power grouting materials' resistance to sulfate acid erosion and chloride ion erosion, but also improves the early strength; and the compound anti-seawater erosion agent can quickly participate in the hydration reaction of cement, play a nucleus role, and reduce the nucleation barrier. The use of anti-seawater erosion agents with micro-nano size can also play a filling role, effectively improving the mechanical properties of offshore wind power grouting materials; in addition, compounded barium salt-doped silica aerogel, the introduction of silica aerogel can fill the pores of concrete and improve its density, and the doped barium salt can not only improve the compressive strength, but also absorb sulfate ions in seawater to generate water-insoluble barium sulfate, which is further filled in the pores of concrete to improve the density and water tightness, thereby significantly improving the durability of offshore wind power grouting materials.
[0008] Furthermore, the barium salt-doped silica aerogel used in the grouting material of the present invention is prepared by the following steps: after the silicon source and the acid are mixed and filtered, they are heated and dried at 120-150° C. in a carbon dioxide atmosphere for 6-8 hours, barium salt is added after cooling, and the barium salt-doped silica aerogel is obtained after crushing; the mass ratio of the silicon source, the acid and the barium salt is 1:(0.5-3):(1-2).
[0009] Furthermore, the silicon source used in the preparation of the barium salt-doped silica aerogel is water glass, tetraethyl orthosilicate or methyl orthosilicate; the acid is sulfuric acid, hydrochloric acid, nitric acid, acetic acid, oxalic acid or phosphoric acid; and the barium salt is barium chloride or barium nitrate.
[0010] Furthermore, the anti-seawater erosion agent used in the grouting material of the present invention includes mineral powder, metakaolin, silica fume, carbon fiber and calcium aluminate crystal nucleus early strength agent in a mass ratio of 1: (0.2-0.3): (0.2-0.3): (0.002-0.005): (0.005-0.008).
[0011] Furthermore, the high-iron phase silicate cement used in the grouting material of the present invention has a strength grade of 52.5, a particle size D50≤6μm, and an iron oxide content of 10-20%.
[0012] Furthermore, the expansion components used in the grouting material of the present invention include calcium sulphoaluminate, iron oxide and dimethylnitrosamide in a mass ratio of 1: (0.3-0.5): (0.001-0.003).
[0013] Furthermore, the fine aggregate used in the grouting material of the present invention includes 10-30 mesh quartz sand, 30-55 mesh quartz sand and 55-100 mesh quartz sand in a mass ratio of 1:(1.2-1.5):(0.5-0.8).
[0014] The method for preparing the above-mentioned offshore wind power grouting material resistant to seawater erosion of the present invention comprises the following steps:
[0015] (1) mixing high iron phase silicate cement, sulphoaluminate cement and fine aggregate to prepare powder A;
[0016] (2) mixing and stirring the seawater erosion resistance agent, the expansion component, the silicon dioxide aerogel doped with barium salt and the water reducing agent to obtain powder B;
[0017] (3) Powder A and powder B are mixed and stirred to prepare an offshore wind power grouting material resistant to seawater erosion.
[0018] Beneficial effects: Compared with the prior art, the significant advantages of the present invention are: the initial fluidity of the grouting material is ≥320mm when applied, and the fluidity of 30min is ≥300mm, which has high fluidity and a long construction time; the 1d compressive strength is ≥80MPa, the 3d compressive strength is ≥125MPa, and the 28d compressive strength is ≥145MPa, which has high early strength and ultra-high strength; the 3h vertical expansion rate is 1.5-2.1%, the difference between the 24h and 3h vertical expansion rates is 0.12-0.%, and the 28d drying shrinkage is 0.12-0.2%, the number of dry-wet cycles of sulphoaluminate is ≥120, and the chloride ion diffusion coefficient is ≤1.0 (10-12m 2 / s), antifreeze performance ≥ F400, excellent resistance to seawater erosion, slight expansion, no shrinkage in the later period, good durability, suitable for grouting materials for offshore wind power infrastructure construction in marine environment. DETAILED DESCRIPTION
[0019] The technical solution of the present invention is further described in detail below in conjunction with embodiments.
[0020] It should be noted that the raw materials used in the present invention can be purchased from the market. Among them, high iron phase silicate cement is purchased from Anhui Conch Group Co., Ltd., and its strength grade is 52.5, and the iron oxide content is 10-20%. Sulfoaluminate cement is purchased from Anhui Conch Group Co., Ltd., and its strength grade is 52.5, 1d compressive strength ≥35MPa, and 3d compressive strength ≥45MPa. The water reducer is a polycarboxylic acid water reducer powder, and the water reduction rate is ≥30%. The calcium sulfonate nucleation early strength agent is mixed with tricalcium aluminate and dihydrate gypsum in a molar ratio of 1:2.5-3.5, and is prepared by a high-energy planetary ball milling-crystallization two-step method, that is, tricalcium aluminate and dihydrate gypsum are wet ball milled for 15-20min to react nucleation, and after crystallization at 60-70°C for 8-12h, the calcium sulfonate nucleation inducer is obtained by filtering, rinsing, drying and ball milling. In addition, the mineral powder used in the anti-seawater erosion agent of the present invention is an ultrafine mineral powder with a particle size D50≤3.0 μm.
[0021] Example 1
[0022] The raw materials used in the seawater erosion-resistant offshore wind power grouting material of this embodiment are shown in Table 1 below.
[0023] Table 1 Raw material composition used in Example 1
[0024]
[0025]
[0026] The raw material components of the anti-seawater corrosion agent are shown in Table 2 below.
[0027] Table 2 Raw material composition of the anti-seawater erosion agent used in Example 1
[0028] raw material Ultrafine mineral powder Metakaolin Silica Fume Carbon Fiber Calcium Sulfate Crystal Nucleus Early Strength Agent Content / kg 1 0.2 0.3 0.002 0.005
[0029] The preparation method of silicon dioxide aerogel doped with barium chloride in the offshore wind power grouting material comprises the following steps: mixing water glass and hydrochloric acid, filtering, heating and drying at 130° C. for 7 hours in a carbon dioxide atmosphere, adding barium chloride after cooling, and crushing to obtain silicon dioxide aerogel doped with barium chloride; wherein the mass ratio of water glass, hydrochloric acid and barium chloride is 1:1.5:4.
[0030] The method for preparing the seawater erosion resistance agent in the offshore wind power grouting material comprises the following steps:
[0031] (1) Mix and homogenize ultrafine mineral powder, metakaolin and silica fume in proportion;
[0032] (2) Grinding in a jet mill for 3 hours, then adding carbon fiber and calcium vanadium crystal nucleus early strength agent and grinding for 1 hour;
[0033] (3) The powder after grinding is sorted by an ultra-fine sorting machine to produce an anti-seawater erosion agent with a particle size of D 50 ≤2μm.
[0034] The method for preparing the offshore wind power grouting material resistant to seawater erosion in this embodiment comprises the following steps:
[0035] (1) mixing high iron phase silicate cement, sulphoaluminate cement and fine aggregate to prepare powder A;
[0036] (2) mixing and stirring the seawater erosion resistance agent, the expansion component, the silicon dioxide aerogel doped with barium chloride and the water reducing agent to obtain powder B;
[0037] (3) Powder A and powder B are mixed and stirred to prepare an offshore wind power grouting material resistant to seawater erosion.
[0038] Example 2
[0039] The raw materials used in the seawater erosion-resistant offshore wind power grouting material of this embodiment are shown in Table 3 below.
[0040] Table 3 Raw material composition used in Example 2
[0041]
[0042]
[0043] The raw material components of the anti-seawater corrosion agent are shown in Table 4 below.
[0044] Table 4 Raw material composition of the anti-seawater erosion agent used in Example 2
[0045] raw material Ultrafine mineral powder Metakaolin Silica Fume Carbon Fiber Calcium Sulfate Crystal Nucleus Early Strength Agent Content / kg 1 0.2 0.2 0.003 0.006
[0046] The preparation method of silicon dioxide aerogel doped with barium chloride in the offshore wind power grouting material comprises the following steps: after tetraethyl orthosilicate and nitric acid are mixed and filtered, they are heated and dried at 140° C. for 7 hours in a carbon dioxide atmosphere, barium chloride is added after cooling, and the silicon dioxide aerogel doped with barium chloride is obtained after crushing; wherein the mass ratio of tetraethyl orthosilicate, nitric acid and barium chloride is 1:2.5:3.5.
[0047] The preparation method of the anti-seawater corrosion agent in the offshore wind power grouting material is the same as that in Example 1.
[0048] The method for preparing the offshore wind power grouting material resistant to seawater erosion in this embodiment comprises the following steps:
[0049] (1) mixing high iron phase silicate cement, sulphoaluminate cement and fine aggregate to prepare powder A;
[0050] (2) mixing and stirring the seawater erosion resistance agent, the expansion component, the silicon dioxide aerogel doped with barium chloride and the water reducing agent to obtain powder B;
[0051] (3) Powder A and powder B are mixed and stirred to prepare an offshore wind power grouting material resistant to seawater erosion.
[0052] Example 3
[0053] The raw materials used in the seawater erosion-resistant offshore wind power grouting material of this embodiment are shown in Table 5 below.
[0054] Table 5 Raw material composition used in Example 3
[0055]
[0056]
[0057] The raw material components of the anti-seawater corrosion agent are shown in Table 5 below.
[0058] Table 5 Raw material composition of the anti-seawater erosion agent used in Example 3
[0059] raw material Ultrafine mineral powder Metakaolin Silica Fume Carbon Fiber Calcium Sulfate Crystal Nucleus Early Strength Agent Content / kg 1 0.2 0.3 0.003 0.006
[0060] The preparation method of silicon dioxide aerogel doped with barium nitrate in the offshore wind power grouting material comprises the following steps: methyl orthosilicate and acetic acid are mixed and filtered, and then heated and dried at 120° C. for 8 hours in a carbon dioxide atmosphere, and barium nitrate is added after cooling, and the silicon dioxide aerogel doped with barium nitrate is obtained after crushing; wherein the mass ratio of methyl orthosilicate, acetic acid and barium nitrate is 1:0.5:3.
[0061] The preparation method of the anti-seawater corrosion agent in the offshore wind power grouting material is the same as that in Example 1.
[0062] The preparation method of the offshore wind power grouting material resistant to seawater erosion in this embodiment is the same as that in Example 1
[0063] Example 4
[0064] The raw materials used in the seawater erosion-resistant offshore wind power grouting material of this embodiment are shown in Table 7 below.
[0065] Table 7 Raw material composition used in Example 4
[0066]
[0067]
[0068] The raw material components of the anti-seawater corrosion agent are shown in Table 8 below.
[0069] Table 8 Raw material composition of the anti-seawater erosion agent used in Example 4
[0070] raw material Ultrafine mineral powder Metakaolin Silica Fume Carbon Fiber Calcium Sulfate Crystal Nucleus Early Strength Agent Content / kg 1 0.2 0.3 0.004 0.007
[0071] The preparation method of silicon dioxide aerogel doped with barium chloride in the offshore wind power grouting material comprises the following steps: methyl orthosilicate and oxalic acid are mixed and filtered, and then heated and dried at 150° C. for 6 hours in a carbon dioxide atmosphere, and barium chloride is added after cooling, and the silicon dioxide aerogel doped with barium chloride is obtained after crushing; wherein the mass ratio of methyl orthosilicate, acetic acid and barium nitrate is 1:3:5.
[0072] The preparation method of the anti-seawater corrosion agent in the offshore wind power grouting material is the same as that in Example 1.
[0073] The preparation method of the offshore wind power grouting material resistant to seawater erosion in this embodiment is the same as that in Example 1.
[0074] Example 5
[0075] The raw materials used in the seawater erosion-resistant offshore wind power grouting material of this embodiment are shown in Table 9 below.
[0076] Table 9 Raw material composition used in Example 4
[0077]
[0078]
[0079] Among them, the raw material components of the anti-seawater corrosion agent are shown in Table 10 below.
[0080] Table 10 Raw material composition of the anti-seawater erosion agent used in Example 5
[0081] raw material Ultrafine mineral powder Metakaolin Silica Fume Carbon Fiber Calcium Sulfate Crystal Nucleus Early Strength Agent Content / kg 1 0.3 0.2 0.005 0.008
[0082] The preparation method of the silicon dioxide aerogel doped with barium chloride in the offshore wind power grouting material is the same as that in Example 1.
[0083] The preparation method of the anti-seawater corrosion agent in the offshore wind power grouting material is the same as that in Example 1.
[0084] The preparation method of the offshore wind power grouting material resistant to seawater erosion in this embodiment is the same as that in Example 1.
[0085] Example 6
[0086] The raw materials used in the seawater erosion-resistant offshore wind power grouting material of this embodiment are shown in Table 11 below.
[0087] Table 11 Raw material composition used in Example 6
[0088]
[0089]
[0090] Among them, the raw material components of the anti-seawater corrosion agent are shown in Table 12 below.
[0091] Table 12 Raw material composition of the anti-seawater erosion agent used in Example 6
[0092] raw material Ultrafine mineral powder Metakaolin Silica Fume Carbon Fiber Calcium Sulfate Crystal Nucleus Early Strength Agent Content / kg 1 0.3 0.3 0.005 0.008
[0093] The preparation method of the silicon dioxide aerogel doped with barium chloride in the offshore wind power grouting material is the same as that in Example 1.
[0094] The preparation method of the anti-seawater corrosion agent in the offshore wind power grouting material is the same as that in Example 1.
[0095] The preparation method of the offshore wind power grouting material resistant to seawater erosion in this embodiment is the same as that in Example 1.
[0096] Comparative Example 1
[0097] The basic steps are the same as those in Example 6, except that no anti-seawater corrosion agent is added, as shown in Table 13 below.
[0098] Table 13 Raw material composition used in comparative example 1
[0099]
[0100] Comparative Example 2
[0101] The basic steps are the same as those in Example 6, except that mineral powder is used instead of the anti-seawater corrosion agent, as shown in Table 14 below.
[0102] Table 14 Raw material composition used in comparative example 2
[0103]
[0104] Comparative Example 3
[0105] The basic steps are the same as those of Example 6, except that ordinary Portland cement is used instead of high iron phase Portland cement and sulphoaluminate cement, as shown in Table 15 below.
[0106] Table 15 Raw material composition used in comparative example 3
[0107]
[0108]
[0109] Comparative Example 4
[0110] The basic steps are the same as those in Example 6, except that barium chloride is directly used instead of silicon dioxide aerogel doped with barium chloride, as shown in Table 16 below.
[0111] Table 16 Raw material composition used in comparative example 4
[0112]
[0113] Performance Testing
[0114] The grouting materials of Examples 1-6 and Comparative Examples 1-4 were prepared into samples and subjected to performance tests. The results obtained are shown in Table 17 below.
[0115] Table 17 Performance results of offshore wind power grouting materials resistant to seawater erosion
[0116]
[0117]
[0118] As can be seen from the table, the initial fluidity of the offshore wind power grouting material resistant to seawater erosion prepared by the present invention is ≥290mm, the fluidity is ≥300mm in 30min, and the fluidity is good; the 1d compressive strength is ≥70MPa, the 3d compressive strength is ≥118MPa, and the 28d compressive strength is ≥142MPa, which has the advantage of ultra-high strength, the 3h vertical expansion rate is 2.1-2.4%, the difference between the 24h and 3h vertical expansion rates is 0.20-0.25%, the early micro-expansion, the permeability reaches P25, and the water tightness is good. Compared with the comparative example, it can be found that the addition of anti-seawater inhibitor significantly improves the number of dry-wet cycles and chloride ion diffusion coefficient of the offshore wind power grouting material; at the same time, the addition of silicon dioxide aerogel doped with barium chloride can significantly improve the permeability and water tightness of the offshore wind power grouting material.
Claims
1. An offshore wind power grouting material resistant to seawater erosion, characterized in that: The raw materials include the following by weight: 40-45 parts of high-iron phase silicate cement, 5-10 parts of sulphoaluminate cement, 5-10 parts of seawater erosion resistance agent, 5-10 parts of expansion component, 34-42 parts of fine aggregate, 0.5-1 parts of silicon dioxide aerogel doped with barium salt, and 0.4-0.5 parts of water reducing agent.
2. The offshore wind power grouting material resistant to seawater erosion according to claim 1 is characterized in that: The barium salt-doped silica aerogel is prepared by the following steps: mixing a silicon source and an acid, filtering the mixture, heating and drying the mixture at 120-150° C. for 6-8 hours in a carbon dioxide atmosphere, adding a barium salt after cooling, and crushing the mixture to obtain the barium salt-doped silica aerogel; the mass ratio of the silicon source, the acid, and the barium salt is 1:(0.5-3):(3-5).
3. The offshore wind power grouting material resistant to seawater erosion according to claim 2 is characterized in that: The silicon source is water glass, tetraethyl orthosilicate or methyl orthosilicate; the acid is hydrochloric acid, nitric acid, acetic acid, oxalic acid or phosphoric acid; and the barium salt is barium chloride or barium nitrate.
4. The offshore wind power grouting material resistant to seawater erosion according to claim 1, characterized in that: The anti-seawater erosion agent comprises mineral powder, metakaolin, silica fume, carbon fiber and ettringite crystal nucleus early strength agent in a mass ratio of 1: (0.2-0.3): (0.2-0.3): (0.002-0.005): (0.005-0.008).
5. The offshore wind power grouting material resistant to seawater erosion according to claim 1, characterized in that: The strength grade of the high iron phase silicate cement is 52.5, wherein the iron oxide content reaches 10-20%.
6. The offshore wind power grouting material resistant to seawater erosion according to claim 1, characterized in that: The expansion component comprises calcium sulphoaluminate, iron oxide and dimethylnitrosamide in a mass ratio of 1:(0.3-0.5):(0.001-0.003).
7. The offshore wind power grouting material resistant to seawater erosion according to claim 1, characterized in that: The fine aggregate includes 10-30 mesh quartz sand, 30-55 mesh quartz sand and 55-100 mesh quartz sand in a mass ratio of 1:(1.2-1.5):(0.5-0.8).
8. A method for preparing the offshore wind power grouting material resistant to seawater erosion according to claim 1, characterized in that: The steps include: (1) mixing high iron phase silicate cement, sulphoaluminate cement and fine aggregate to prepare powder A; (2) mixing and stirring the seawater erosion resistance agent, the expansion component, the silicon dioxide aerogel doped with barium salt and the water reducing agent to obtain powder B; (3) Powder A and powder B are mixed and stirred to prepare an offshore wind power grouting material resistant to seawater erosion.
Citation Information
Cited By
Grouting material for offshore wind power jacket as well as preparation method and application of grouting material
CN121517161A