Silanized hydrogenated polybutadiene as well as preparation method and application thereof

By silanizing and catalyzed hydrotreating polybutadiene improves its adsorption and lubricating properties with metals, the problem of insufficient performance of polybutadiene liquid rubber in low temperature and vacuum environments is solved, and a suitable fluid lubricant is prepared silanized hydrogenated polybutadiene.

CN118978621APending Publication Date: 2024-11-19LANZHOU UNIV
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411053829.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Polybutadiene liquid rubber has poor adsorption and poor lubricating properties with metals, resulting in poor performance in low-temperature fluidity and vacuum environments.

Method used

By silanizing and catalyzed hydrotreating polybutadiene, a silaned hydrogenated polybutadiene containing a specific repeating unit structure is prepared, which changes its polarity and structure, thereby improving its metal adsorption capacity and lubricating properties. The specific steps include silanization reaction with 5% chloroplatinic acid as a catalyst and n-heptane as solvent under anhydrous and anaerobic conditions, and then catalytic hydrotreatment with 5% palladium carbon as catalyst in an autoclave.

Benefits of technology

It reduces the glass transition temperature of polybutadiene, expands its low-temperature usage temperature range, improves its polarity and lubricating properties, and makes it perform better in low-temperature and low-vacuum environments. It is suitable for fluid lubricants. Especially space heavy loading of long-life moving parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention provides silanized hydrogenated polybutadiene as well as a preparation method and application thereof. The silanized hydrogenated polybutadiene is prepared by carrying out addition on triethyl silane and polybutadiene by taking an isopropanol solution of chloroplatinic acid as a catalyst under anhydrous and anaerobic conditions, and then carrying out catalytic hydrogenation. The silanized hydrogenated polybutadiene is prepared by taking silanized 1, 2-butadiene, 1, 2-butadiene and 1, 4-butadiene as repetitive units, side groups of the silanized hydrogenated polybutadiene are provided with silyl groups, and double bonds in molecular chains of the silanized hydrogenated polybutadiene are subjected to hydrogenation treatment. The silanized hydrogenated polybutadiene has the advantages of favorable wear resistance, low vacuum volatility and favorable low-temperature fluidity, and is suitable for being used as a fluid lubricant for spatial heavy-load long-life moving parts.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lubricant preparation, and in particular to silylated hydrogenated polybutadiene and a preparation method and application thereof. Background Art

[0002] Polybutadiene rubber is an important liquid rubber, which is synthesized by various polymerization methods with butadiene as monomer. It has the advantages of excellent cold resistance, good thermal stability, easy processing, good low-temperature fluidity, etc., and is widely used in tire manufacturing, copolymer resin synthesis, sealing rings, adhesives and other industries.

[0003] Polybutadiene contains double bonds, which can be added to carry functional groups. In patent document CN103797036A, polybutadiene is silylated and mixed with a polymerization initiator to prepare a curable composition, and a cured product with high shear force is obtained by utilizing the interaction between the unsaturated double bonds in the silylated polybutadiene and the polymerization initiator.

[0004] Polybutadiene liquid rubber has good low-temperature fluidity, but it is a weakly polar polymer, which results in poor strength of the fluid film it forms and weak adsorption to the metal matrix.

[0005] In order to effectively improve the problems of poor metal adsorption and poor lubrication performance of hydrogenated polybutadiene, providing a fluid lubricant with good low-temperature fluidity, excellent lubricity and low vacuum volatility has become a technical problem that needs to be urgently solved by technicians in this field. Summary of the invention

[0006] Therefore, the technical problem to be solved by the present invention is to overcome the problems of poor adsorption of polybutadiene liquid rubber to metal and poor lubrication performance in the prior art, thereby providing a silylated hydrogenated polybutadiene with low vacuum volatility, good low-temperature fluidity and excellent lubricity, and a preparation method and application thereof.

[0007] To achieve the above object, the present invention provides the following technical solutions:

[0008] In a first aspect, the present invention provides a silylated hydrogenated polybutadiene comprising two repeating units represented by formula (a), formula (b) and formula (c) in formula (1), wherein both the main chain and the side groups thereof are saturated structures,

[0009]

[0010] In formula (a), formula (b) and formula (c), R1, R2 and R3 are each independently ethyl or isopropyl.

[0011] Furthermore, in terms of molar percentage, the silylated hydrogenated polybutadiene molecule contains 1% to 50% of the repeating unit represented by the formula (a), and the rest are the repeating units represented by the formula (b) or the repeating units represented by the formula (c).

[0012] Furthermore, in the silylated hydrogenated polybutadiene molecule, the sum of the repeating unit represented by the formula (a) and the repeating unit represented by the formula (b) is 75% to 100%, and the repeating unit represented by the formula (c) is 0% to 25% by mole percentage.

[0013] Furthermore, the silylated hydrogenated polybutadiene is obtained by silylation of polybutadiene followed by catalytic hydrogenation.

[0014] Furthermore, the number average molecular weight of the polybutadiene is 2437-4232 g / mol.

[0015] In a second aspect, the present invention provides a method for preparing the silylated hydrogenated polybutadiene, comprising the following steps:

[0016] Step 1: Silanization

[0017] Under anhydrous and oxygen-free conditions, using 5% chloroplatinic acid isopropanol solution as a catalyst and n-heptane as a solvent, triethylsilane and polybutadiene are reacted at a mass ratio of 11:50 to 1:1 at 90 to 110° C. for 6 to 18 hours to obtain silylated polybutadiene;

[0018] Step 2: Catalytic hydrogenation

[0019] The silylated polybutadiene obtained in step 1 is transferred to a high-pressure reactor, 5% palladium carbon is used as a catalyst, n-heptane is used as a solvent, the gas in the reactor is replaced with hydrogen and pressurized to 4-6 MPa, and the reaction is carried out at 100-120° C. for 10-12 hours to obtain silylated hydrogenated polybutadiene.

[0020] In a third aspect, the present invention provides use of the silylated hydrogenated polybutadiene in the preparation of a fluid lubricant.

[0021] The technical solution of the present invention has the following advantages:

[0022] The present invention reduces the glass transition temperature of polybutadiene liquid rubber through silylation and catalytic hydrogenation, thereby widening its low-temperature use temperature range, and changes the polarity of polybutadiene liquid rubber to make it more polar and more excellent in lubrication performance. In addition, the structure of polybutadiene is similar to that of existing poly-α-olefin lubricating oil, and after silylation and catalytic hydrogenation treatment, the comprehensive performance of silylated hydrogenated polybutadiene, such as metal adsorption capacity, volatility, and lubrication performance, is more excellent.

[0023] The silylated hydrogenated polybutadiene of the invention has good low-temperature fluidity, low vacuum volatility and excellent lubricity, and is particularly suitable for fluid lubrication applications of heavy-loaded and long-life moving parts in space. DETAILED DESCRIPTION

[0024] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.

[0025] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the art can be used. The raw materials or instruments used are all conventional products that can be obtained commercially, including but not limited to the raw materials or instruments used in the examples of this application.

[0026] The silylated hydrogenated polybutadiene of the present application contains two repeating units represented by formula (a), formula (b) and formula (c) in formula (1), and the main chain and side groups thereof are both saturated structures.

[0027]

[0028] In formula (a), formula (b) and formula (c), R1, R2 and R3 are each independently ethyl or isopropyl.

[0029] The silylated hydrogenated polybutadiene molecule of the present application contains, by mole percentage, 1% to 50% of the repeating unit represented by formula (a), and the rest are the repeating units represented by formula (b) or the repeating units represented by formula (c).

[0030] In the silylated hydrogenated polybutadiene molecule of the present application, the sum of the repeating units represented by formula (a) and the repeating units represented by formula (b) is 75% to 100% by mole, and the repeating units represented by formula (c) is 0% to 25%.

[0031] The silylated hydrogenated polybutadiene of the present application is obtained by silylation of polybutadiene and then catalytic hydrogenation, wherein the number average molecular weight of the polybutadiene is 2437-4232 g / mol.

[0032] The silylated hydrogenated polybutadiene and the preparation method thereof of the present application are described in the following examples.

[0033] Example 1

[0034] This embodiment provides a method for preparing silylated hydrogenated polybutadiene, and the specific steps are as follows:

[0035] Step 1: Silanization

[0036] Under anhydrous and oxygen-free conditions, using 5% chloroplatinic acid isopropanol solution as a catalyst and n-heptane as a solvent, 8.8 g of triethylsilane and 40 g of polybutadiene with a number average molecular weight of 3103 g / mol (mass ratio of 11:50) were reacted at 110° C. for 6 h to obtain silylated polybutadiene;

[0037] Step 2: Catalytic hydrogenation

[0038] The silylated polybutadiene obtained in step 1 was transferred to a high-pressure reactor, 5% palladium carbon was used as a catalyst, n-heptane was used as a solvent, the gas in the reactor was replaced with hydrogen and pressurized to 4 MPa, and the reaction was carried out at 120° C. for 12 hours to obtain silylated hydrogenated polybutadiene.

[0039] According to the measurement by nuclear magnetic resonance spectroscopy, in this embodiment, the addition amount of triethylsilane is 6.3%.

[0040] Example 2

[0041] This embodiment provides a method for preparing silylated hydrogenated polybutadiene. The steps and process parameters thereof can be referred to in Example 1, except that the silylation reaction time is 12 hours.

[0042] According to the measurement by nuclear magnetic resonance spectrum, in this embodiment, the addition amount of triethylsilane is 9.0%.

[0043] Example 3

[0044] This embodiment provides a method for preparing silylated hydrogenated polybutadiene. The steps and process parameters thereof can be referred to in Example 1, except that the silylation reaction time is 18 hours.

[0045] According to the nuclear magnetic resonance spectrum, in this embodiment, the amount of triethylsilane added is 9.2% (numbered HLBR-3K-10%).

[0046] Example 4

[0047] This embodiment provides a method for preparing silylated hydrogenated polybutadiene, and the specific steps are as follows:

[0048] Step 1: Silanization

[0049] Under anhydrous and oxygen-free conditions, using 5% chloroplatinic acid isopropanol solution as a catalyst and n-heptane as a solvent, 17.2 g of triethylsilane and 40 g of polybutadiene with a number average molecular weight of 3103 g / mol (mass ratio of 43:100) were reacted at 110° C. for 12 h to obtain silylated polybutadiene;

[0050] Step 2: Catalytic hydrogenation

[0051] The silylated polybutadiene obtained in step 1 was transferred to a high-pressure reactor, 5% palladium carbon was used as a catalyst, n-heptane was used as a solvent, the gas in the reactor was replaced with hydrogen and pressurized to 4 MPa, and the reaction was carried out at 120° C. for 12 hours to obtain silylated hydrogenated polybutadiene.

[0052] According to the nuclear magnetic resonance spectrum, in this embodiment, the amount of triethylsilane added is 19.2% (numbered HLBR-3K-20%).

[0053] Example 5

[0054] This embodiment provides a method for preparing silylated hydrogenated polybutadiene, and its steps and process parameters can refer to Example 4, except that: the raw materials for the silylation reaction are: 40g triethylsilane and 40g polybutadiene with a number average molecular weight of 3103g / mol (mass ratio is 1:1).

[0055] According to the measurement by nuclear magnetic resonance spectroscopy, in this embodiment, the addition amount of triethylsilane is 30.68% (numbered as HLBR-3K-30%).

[0056] Example 6

[0057] This embodiment provides a method for preparing silylated hydrogenated polybutadiene, and its steps and process parameters can refer to Example 4, except that: the raw materials for the silylation reaction are: 40g triethylsilane and 40g polybutadiene with a number average molecular weight of 3103g / mol (mass ratio is 1:1).

[0058] According to the measurement by nuclear magnetic resonance spectroscopy, in this embodiment, the addition amount of triethylsilane is 38.4% (numbered as HLBR-3K-30%).

[0059] Example 7

[0060] This embodiment provides a method for preparing silylated hydrogenated polybutadiene, and the specific steps are as follows:

[0061] Step 1: Silanization

[0062] Under anhydrous and oxygen-free conditions, using 5% chloroplatinic acid isopropanol solution as a catalyst and n-heptane as a solvent, 40 g of triethylsilane and 40 g of polybutadiene with a number average molecular weight of 2437 g / mol (mass ratio of 1:1) are reacted at 110° C. for 12 h to obtain silylated polybutadiene;

[0063] Step 2: Catalytic hydrogenation

[0064] The silylated polybutadiene obtained in step 1 was transferred to a high-pressure reactor, 5% palladium carbon was used as a catalyst, n-heptane was used as a solvent, the gas in the reactor was replaced with hydrogen and pressurized to 4 MPa, and the reaction was carried out at 120° C. for 12 hours to obtain silylated hydrogenated polybutadiene.

[0065] According to the nuclear magnetic resonance spectrum, in this embodiment, the amount of triethylsilane added is 19.2% (numbered HLBR-2K-20%).

[0066] Example 8

[0067] This embodiment provides a method for preparing silylated hydrogenated polybutadiene, and its steps and process parameters can refer to Example 4, except that: the raw materials for the silylation reaction are: 40g triethylsilane and 40g polybutadiene with a number average molecular weight of 3103g / mol (mass ratio is 1:1).

[0068] According to the nuclear magnetic resonance spectrum, in this embodiment, the amount of triethylsilane added is 19.2% (numbered HLBR-4K-20%).

[0069] Test Case

[0070] The glass transition temperature and wear resistance of the silylated hydrogenated polybutadiene prepared in Examples 1 to 8 were tested.

[0071] Glass transition temperature test: The glass transition temperature of silylated hydrogenated polybutadiene prepared under different synthesis conditions was tested by a synchronous thermal analyzer. The test results are shown in Table 1.

[0072] Anti-wear performance test: A four-ball friction tester was used to test the anti-wear performance of silanized hydrogenated polybutadiene prepared under different synthesis conditions. Test conditions: steel ball diameter 9.525mm, load 200N, rotation speed 100rpm, continuous friction for 1h, room temperature environment. After the friction test, the surface profiler was used to test the wear spot diameters of the three steel ball surfaces and the average value was calculated. The test results are shown in Table 1.

[0073] Table 1 Glass transition temperature and tribological properties test results

[0074]

[0075]

[0076] It can be seen from Table 1 that after polybutadiene liquid rubber is treated with silanization, the glass transition temperature is reduced, which will widen its low-temperature use temperature range as a fluid lubricant. After polybutadiene is treated with silanization and hydrogenation, the average vacuum four-ball wear spot diameter of polybutadiene is much lower than the average vacuum four-ball wear spot diameter of polybutadiene liquid rubber, and the wear resistance is effectively improved, with more excellent wear resistance.

[0077] In summary, by silylation and catalytic hydrogenation of polybutadiene liquid rubber, the glass transition temperature of polybutadiene liquid rubber is reduced, the low-temperature use temperature range is widened, and at the same time, the polarity is changed to be higher and the lubrication performance is better. After polybutadiene is silylated and hydrogenated, the comprehensive performances of silylated hydrogenated polybutadiene, such as metal adsorption capacity, vacuum volatility, lubricity, and wear resistance, are more excellent. Therefore, the silylated hydrogenated polybutadiene of the present application has good low-temperature fluidity, low vacuum volatility, and excellent lubricity, and is particularly suitable for fluid lubrication applications of heavy-loaded and long-life moving parts in space.

[0078] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.

Claims

1. A silylated hydrogenated polybutadiene, characterized in that: The silylated hydrogenated polybutadiene contains two repeating units represented by formula (a), formula (b) and formula (c) in formula (1), and the main chain and side groups thereof are both saturated structures. In formula (a), formula (b) and formula (c), R1, R2 and R3 are each independently ethyl or isopropyl.

2. The silylated hydrogenated polybutadiene according to claim 1, characterized in that: In terms of molar percentage, the silylated hydrogenated polybutadiene molecule contains 1% to 50% of the repeating unit represented by the formula (a), and the rest are the repeating units represented by the formula (b) or the repeating units represented by the formula (c).

3. The silylated hydrogenated polybutadiene according to any one of claims 1 to 2, characterized in that: In terms of molar percentage, in the silylated hydrogenated polybutadiene molecule, the sum of the repeating unit represented by the formula (a) and the repeating unit represented by the formula (b) is 75% to 100%, and the repeating unit represented by the formula (c) is 0% to 25%.

4. The silylated hydrogenated polybutadiene according to any one of claims 1 to 3, characterized in that: The polybutadiene is obtained by silylation and then catalytic hydrogenation, wherein the number average molecular weight of the polybutadiene is 2437-4232 g / mol.

5. The method for preparing silylated hydrogenated polybutadiene according to any one of claims 1 to 4, characterized in that: The following steps are involved: Step 1: Silanization Under anhydrous and oxygen-free conditions, using 5% chloroplatinic acid isopropanol solution as a catalyst and n-heptane as a solvent, triethylsilane and polybutadiene are reacted at a mass ratio of 11:50 to 1:1 at 90 to 110° C. for 6 to 18 hours to obtain silylated polybutadiene; Step 2: Catalytic hydrogenation The silylated polybutadiene obtained in step 1 is transferred to a high-pressure reactor, 5% palladium carbon is used as a catalyst, n-heptane is used as a solvent, the gas in the reactor is replaced with hydrogen and pressurized to 4-6 MPa, and the reaction is carried out at 100-120° C. for 10-12 hours to obtain silylated hydrogenated polybutadiene.

6. Use of the silylated hydrogenated polybutadiene according to any one of claims 1 to 5 in the preparation of a fluid lubricant.

Citation Information

Patent Citations

  • Silylated polybutadiene

    CN103797036A

  • Tire member, hydrogenated conjugated diene polymer and polymer composition

    CN105026484A

  • Method for manufacturing hydrogenated polymer

    CN106795231A

  • Hydrogenated polybutadienes useful as lubricant additives

    CN108503741A

  • Process for preparing epoxy-terminated polymers

    CN1086522A