3D printing ink based on dynamic hydrogel, preparation method and application of 3D printing ink in transition metal sulfide three-dimensional material

Through dynamic hydrogel ink printing technology, the problem of TMDs material printing is solved, the three-dimensional structural printing and electrocatalytic activity of TMDs material are realized, and a new additive manufacturing method for TMDs material is provided.

CN118978634AInactive Publication Date: 2024-11-19YANGTZE DELTA REGION INST OF UNIV OF ELECTRONICS SCI & TECH OF CHINE (HUZHOU)
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411465381.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-21
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The prior art lacks direct-print printing inks that can be used to print transition metal sulfide (TMDs)-based materials, limiting the additive manufacturing of TMDs materials.

Method used

Using dynamic hydrogel-based 3D printing ink, a hydrophobic interaction environment is formed by mixing surfactant, hydrophobic monomer and acrylamide monomer, a hydrophobic interaction environment is formed, and crosslinking agents and initiators are added to form ink, and 3D printing technology is used. The preset structure is printed out and stabilized in the metal salt solution, followed by freeze-drying and calcining to convert to the TMDs three-dimensional material.

Benefits of technology

The TMDs material with complex three-dimensional structures is realized by using direct ink writing technology, providing a new additive manufacturing method for TMDs materials, and has the electrocatalytic activity of oxygen precipitation reaction and hydrogen precipitation reaction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978634A_ABST
    Figure CN118978634A_ABST
Patent Text Reader

Abstract

The invention discloses 3D printing ink based on dynamic hydrogel, a preparation method of the 3D printing ink and application of the 3D printing ink in transition metal sulfide three-dimensional materials, and belongs to the technical field of additive manufacturing. The preparation method of the 3D printing ink comprises the following steps: (1) dissolving a proper amount of surfactant in a sodium chloride aqueous solution, and heating to form a micelle solution; (2) adding a hydrophobic monomer and an acrylamide monomer into the micelle solution, and carrying out ultrasonic treatment until the solution becomes transparent; and (3) cooling to room temperature, sequentially adding a cross-linking agent and an initiator, and standing for reaction to form the 3D printing ink based on the dynamic hydrogel. The self-supported transition metal sulfide skeleton is prepared from the 3D printing ink, has the characteristics of high porosity, high flux, high oxidation-reduction electro-catalysis performance and the like, is simple in preparation method, is suitable for an electro-catalyst carrier and a photocatalyst carrier, and has a relatively high application prospect in the fields of electro-catalysis, sewage treatment and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of hydrogel preparation, and specifically relates to the preparation of a 3D printable ink based on dynamic micellar hydrogel, which can be used as a precursor to print transition metal sulfur compound three-dimensional materials, and has electrocatalytic reaction activity of oxygen evolution reaction (OER) and hydrogen evolution reaction (HER). Background Art

[0002] Transition metal disulfides (TMDs) have good mechanical properties, high carrier mobility and excellent thermal conductivity, and have great application potential in many fields such as field effect transistors, batteries and optoelectronic devices. By customizing the three-dimensional geometric structure of TMDs materials, their application performance can be further improved and their application range can be expanded. For example, constructing a regular and ordered porous channel structure can increase the surface area of ​​TMDs-based electrocatalysts, promote material transport during water electrolysis, and improve its chemical reaction efficiency.

[0003] 3D printing technology is the most effective means to construct specific three-dimensional structural materials. At present, a variety of 3D printing technologies have been developed to adapt to different material systems, such as fused deposition modeling, stereolithography, digital light processing, selective laser sintering, etc. Among them, direct ink writing (DIW) has attracted much attention due to its simple operation, strong adaptability and high cost-effectiveness. DIW technology is an extrusion-based 3D printing technology that uses non-Newtonian viscous slurry as ink to build 3D structures by stacking layer by layer. Paste ink is the key to successful printing. In order to adapt to the printing preparation process and maintain the support capacity of the shape after printing, the ink must have the properties of shear thinning and solidification transition. Therefore, polymers containing multivalent non-covalent or dynamic covalent interaction groups are usually used as design materials for inks, such as metal ligand coordination polymer networks, hydrogen bond networks, electrostatic interaction networks, and hydrophobic interaction networks. However, the above polymers rarely use sulfur and transition metal elements as building matrices, and sulfur and transition metal elements are precursors that can eventually be converted into TMDs-based materials, which poses a challenge to the additive manufacturing of TMDs-based materials using DIW technology.

[0004] Through the above analysis, the problems and defects of the prior art are: lack of direct-write printing ink that can be used to print TMDs-based materials. Summary of the invention

[0005] In view of the problems existing in the background technology, the purpose of the present invention is to provide a 3D printable ink based on dynamic hydrogel, a preparation method and its application in transition metal sulfide three-dimensional materials.

[0006] In order to achieve the above technical objectives, the present invention adopts the following technical solutions: A method for preparing a 3D printable ink based on dynamic hydrogel comprises the following steps: (1) Dissolve an appropriate amount of surfactant in a sodium chloride aqueous solution and heat to form a micellar solution.

[0007] (2) Add hydrophobic monomer and acrylamide monomer to the micelle solution and treat by ultrasonication until the solution becomes transparent.

[0008] (3) After cooling to room temperature, a cross-linking agent and an initiator are added in sequence and allowed to react to form a dynamic hydrogel-based 3D printable ink.

[0009] Preferably, the surfactant in step (1) is sodium dodecyl sulfate, and the heating temperature is 40°C to 60°C.

[0010] Preferably, the hydrophobic monomer in step (2) is one or more of eicosyl methacrylate, octadecyl methacrylate, and dodecyl methacrylate.

[0011] Preferably, the molar ratio of the hydrophobic monomer to the acrylamide monomer in step (2) is 1:220.

[0012] Preferably, in step (3), the cross-linking agent is N,N-methylenebisacrylamide, the initiator is ammonium persulfate, and the catalyst is tetramethylethylenediamine.

[0013] The present invention also provides an application of a 3D printable ink based on a dynamic hydrogel in preparing a transition metal sulfide three-dimensional material. The preparation method of the transition metal sulfide three-dimensional material is characterized by comprising the following steps: Step 1: Load the dynamic hydrogel-based 3D printable ink into a syringe and directly print to form a preset structure.

[0014] Step 2: Immerse the preset structure in a metal salt solution to stabilize the structure and load metal ions at the same time.

[0015] Step three, freeze-drying the formed hydrogel and calcining it at high temperature to transform it to obtain a transition metal sulfide three-dimensional material.

[0016] Preferably, the nominal diameter of the syringe needle in step 1 is 0.5 ~ 1.5 mm, the equipment used is an extrusion 3D printing equipment, and the printing conditions are as follows: printing at room temperature; extrusion pressure is 30 ~ 40 kPa; gun head moving speed: 15 ~ 20 mm / s.

[0017] Preferably, the metal salt solution in step 2 includes one or more of ferric chloride hexahydrate, nickel sulfate heptahydrate, copper sulfate pentahydrate, tin chloride, cobalt sulfate heptahydrate, and lead nitrate, and the concentration of the metal salt solution is 0.1 to 1 mol / L.

[0018] Preferably, the high temperature calcination atmosphere in step three is an argon-hydrogen mixed gas, with the volumes of argon and hydrogen being 95% and 5% respectively; the high temperature calcination temperature is 700-900°C, the heating rate is 5-10°C / min, and then naturally cooled to room temperature.

[0019] In combination with the above technical solutions and the technical problems solved, the advantages and positive effects of the technical solutions to be protected by the present invention are as follows: The hydrophobic interaction-based supramolecular hydrogel is used as a direct-writing 3D printing ink, and TMDs materials with complex three-dimensional structures can be printed. In the hydrogel ink, the micromicelles formed by sodium dodecyl sulfate (SDS) provide a hydrophobic interaction environment between long alkyl chains. It is worth noting that SDS not only acts as a sulfur precursor for the TMDs material, but also provides a carrier for the transition metal element precursor of the material, thereby realizing the introduction of the transition metal element precursor. In addition, the diffused transition metal ions can also form additional interactions with the dodecyl sulfonic acid groups, thereby stabilizing the printed three-dimensional structure. This innovative method provides new ideas and approaches for the additive manufacturing of TMDs materials using DIW technology. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments of the present invention. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0021] Figure 1 : Flow chart of the preparation method of hydrogel ink and printed TMDs three-dimensional material provided by the embodiments of the present invention.

[0022] Figure 2 :Flowchart of the application of dynamic hydrogel-based 3D printable ink in the preparation of transition metal sulfide three-dimensional materials.

[0023] Figure 3 : are state diagrams of the three-dimensional hydrogel after printing in Example 1, wherein Figure 3 (1) is the picture after forming. Figure 3 (2) is the picture after freeze drying. Figure 3 (3) in the figure is the picture after high-temperature calcination.

[0024] Figure 4 : X-ray diffraction patterns of cobalt sulfide, nickel sulfide and ferrous sulfide after calcination.

[0025] Figure 5: Scanning electron microscope (SEM) image of nickel sulfide material after calcination.

[0026] Figure 6 : Electrochemical polarization curves of OER and HER of nickel sulfide materials. DETAILED DESCRIPTION

[0027] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0028] like Figure 1 As shown, in an embodiment of the present invention, a method for preparing a 3D printable ink based on a dynamic hydrogel comprises the following steps: (1) Dissolve an appropriate amount of surfactant in a sodium chloride aqueous solution and heat to form a micellar solution.

[0029] (2) Add hydrophobic monomer and acrylamide monomer to the micelle solution and treat by ultrasonication until the solution becomes transparent.

[0030] (3) After cooling to room temperature, a cross-linking agent and an initiator are added in sequence and allowed to react to form a dynamic hydrogel-based 3D printable ink.

[0031] The surfactant in step (1) is sodium dodecyl sulfate (SDS), and the heating temperature is 40° C. to 60° C. Preferably, the concentration of the NaCl solution used in step (1) is 0.05 to 2 mol / L, and the concentration of the dissolved SDS is 0.2 to 1 mol / L.

[0032] The hydrophobic monomer in step (2) is eicosyl methacrylate (C 20 ), octadecyl methacrylate (C 18 ), dodecyl methacrylate (C 12 ) One or more.

[0033] The hydrophobic monomer and acrylamide monomer C in step (2) 18 The molar ratio to AAm is 1:220.

[0034] C used in step (2) 18 The solution concentration is 3 ~ 5 mmol / L, and the AAm solution concentration is 660~1110 mmol / L.

[0035] In step (3), the cross-linking agent is N,N-methylenebisacrylamide (MBAA), the initiator is ammonium persulfate (APS), and the catalyst is tetramethylethylenediamine (TEMED).

[0036] In step (3), 0.003 to 0.001 g of crosslinking agent N,N-methylenebisacrylamide (MBAA), 0.08 to 0.1 g of initiator ammonium persulfate (APS), and 10 to 30 µL of catalyst tetramethylethylenediamine (TEMED) are added, and the standing time is 12 to 24 hours.

[0037] like Figure 2 As shown, a 3D printable ink based on dynamic hydrogel is used in the preparation of transition metal sulfide three-dimensional materials. The preparation method of the transition metal sulfide three-dimensional material is characterized by comprising the following steps: Step 1: Load the dynamic hydrogel-based 3D printable ink into a syringe and directly print to form a preset structure.

[0038] Step 2: Immerse the preset structure in a metal salt solution to stabilize the structure and load metal ions at the same time.

[0039] Step three, freeze-drying the formed hydrogel and calcining it at high temperature to transform it to obtain a transition metal sulfide three-dimensional material.

[0040] The nominal diameter of the syringe needle described in step 1 is 0.5 ~1.5mm, the equipment used is an extrusion 3D printing equipment, and the printing conditions are as follows: printing at room temperature; extrusion pressure is 30 ~ 40kPa; gun head moving speed: 15 ~ 20mm / s.

[0041] The metal salt solution in step 2 includes one or more of iron (III) chloride hexahydrate (FeCl3·6H2O), nickel (II) sulfate heptahydrate (NiSO4·7H2O), copper (II) sulfate pentahydrate (CuSO4·5H2O), tin (II) chloride (SnCl2), cobalt (II) sulfate heptahydrate (CoSO4·7H2O), and lead nitrate (Pb(NO3)2). The concentration of the metal salt solution is 0.1 to 1 mol / L, and the hydrogel immersion time is 12 to 24 hours.

[0042] In step 3, the freeze-drying time of the three-dimensional hydrogel is 24 to 48 hours.

[0043] The high temperature calcination atmosphere in step 3 is an argon-hydrogen mixed gas, with the volumes of argon and hydrogen being 95% and 5% respectively; the high temperature calcination temperature is 700-900°C, the heating rate is 5-10°C / min, and then naturally cooled to room temperature.

[0044] The freeze-dried hydrogel in step three is transferred to a crucible and then placed in an atmosphere furnace. A hydrogen-argon atmosphere is introduced for protection and a slightly positive pressure is maintained. The mixture is heated to 900°C at 10°C / min and then naturally cooled to room temperature to obtain a transition metal sulfide three-dimensional material.

[0045] The electrocatalytic activity of the above transition metal sulfide three-dimensional materials was tested. The electrochemical test method adopted a three-electrode system. The test electrode was a glassy carbon electrode, the reference electrode was a mercury oxide electrode, and the counter electrode was a platinum electrode. The voltage scanning range for determining hydrogen evolution was -0.8~0 V vs. RHE, and the voltage scanning range for determining oxygen evolution was 1.2 ~ 1.6 V vs. RHE, and a linear sweep voltammetric curve was obtained. The loading amount of the tested electrocatalyst was 0.3 ~ 0.8 g / cm 2 .

[0046] In order to make the disclosure of the present invention more complete, it is described below through more specific embodiments.

[0047] Example 1.

[0048] 1. Dissolve 2.12 g of SDS in 30 ml of 0.8 M NaCl solution at 60°C and stir until completely dissolved to form a micellar solution.

[0049] 2. Add 0.26 g of hydrophobic monomer (such as C 18 ) and sonicate until the solution becomes transparent.

[0050] 3. After cooling to room temperature, add 1.5 g of acrylamide (AAm) monomer and degas with nitrogen for 10 minutes.

[0051] 4. Add 0.003 g of cross-linking agent MBAA, 0.08 g of initiator APS and 10 μl of TEMED in sequence and let stand for 12 hours to form a hydrogel.

[0052] 5. Load the formed hydrogel into a syringe and form a preset 3D structure through injection printing.

[0053] 6. Immerse the printed hydrogel structure in 0.1M nickel sulfate solution for 24 hours to stabilize the structure (see Figure 3 ).

[0054] 7. After freeze drying, the mixture was calcined at 900°C for 2 hours at a heating rate of 10°C / min in a H2 / Ar atmosphere (5% H2 and 95% Ar), and then cooled to room temperature to obtain nickel sulfide. The X-ray diffraction pattern of nickel sulfide is shown in Figure 4 , the scanning electron microscope (SEM) image of the calcined nickel sulfide material is shown in Figure 5 , the electrochemical polarization curves of OER and HER of nickel sulfide materials are shown in Figure 6 .

[0055] Example 2.

[0056] 1. Dissolve 2.12 g of SDS in 30 ml of 0.6 M NaCl solution at 50°C and stir until completely dissolved to form a micellar solution.

[0057] 2. Add 0.26 g of hydrophobic monomer (such as C 18 ) and sonicate until the solution becomes transparent.

[0058] 3. After cooling to room temperature, add 2 g of acrylamide (AAm) monomer and degas with nitrogen for 10 minutes.

[0059] 4. Add 0.001 g of cross-linking agent MBAA, 0.1 g of initiator APS and 20 μl of TEMED in sequence and let stand for 24 hours to form a hydrogel.

[0060] 5. Load the formed hydrogel into a syringe and form a preset 3D structure through injection printing.

[0061] 6. Immerse the printed hydrogel structure in 0.1 M cobalt sulfate solution for 24 hours to stabilize the structure.

[0062] 7. After freeze drying, the mixture was calcined at 800°C for 2 hours at a heating rate of 10°C / min in a H2 / Ar atmosphere (5% H2 and 95% Ar), and then cooled to room temperature to obtain cobalt sulfide. The X-ray diffraction pattern of cobalt sulfide is shown in Figure 4 .

[0063] Example 3.

[0064] 1. Dissolve 2.12 g of SDS in 30 ml of 0.6 M NaCl solution at 50°C and stir until completely dissolved to form a micellar solution.

[0065] 2. Add 0.26 g of hydrophobic monomer (such as C 20 ) and sonicate until the solution becomes transparent.

[0066] 3. After cooling to room temperature, add 2 g of acrylamide (AAm) monomer and degas with nitrogen for 10 minutes.

[0067] 4. Add 0.001 g of cross-linking agent MBAA, 0.1 g of initiator APS and 20 μl of TEMED in sequence and let stand for 24 hours to form a hydrogel.

[0068] 5. Load the formed hydrogel into a syringe and form a preset 3D structure through injection printing.

[0069] 6. Immerse the printed hydrogel structure in 0.1 M ferric chloride solution for 24 hours to stabilize the structure.

[0070] 7. After freeze drying, the mixture was calcined at 800°C for 2 hours at a heating rate of 10°C / min in a H2 / Ar atmosphere (5% H2 and 95% Ar), and cooled to room temperature to obtain ferrous sulfide. The X-ray diffraction pattern of ferrous sulfide is shown in Figure 4 .

[0071] The above three embodiments demonstrate that the composition and structure of TMDs materials can be controlled by controlling the composition of micellar hydrogel ink, the type of metal salt ions, and the calcination conditions. The advantage of this method is that it can prepare TMDs materials with a preset three-dimensional structure, which is suitable for water electrolysis equipment.

[0072] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a 3D printable ink based on dynamic hydrogel, characterized in that: The following steps are involved: (1) Dissolve an appropriate amount of surfactant in a sodium chloride aqueous solution and heat to form a micellar solution; (2) adding a hydrophobic monomer and acrylamide monomer to the micelle solution and ultrasonically treating the solution until the solution becomes transparent; (3) After cooling to room temperature, a cross-linking agent and an initiator are added in sequence and allowed to react to form a dynamic hydrogel-based 3D printable ink.

2. The method for preparing a 3D printable ink based on dynamic hydrogel according to claim 1, characterized in that: The surfactant in step (1) is sodium dodecyl sulfate, and the heating temperature is 40°C to 60°C.

3. The method for preparing a 3D printable ink based on dynamic hydrogel according to claim 1, characterized in that: The hydrophobic monomer in step (2) is one or more of eicosyl methacrylate, octadecyl methacrylate, and dodecyl methacrylate.

4. The method for preparing a 3D printable ink based on dynamic hydrogel according to claim 1, characterized in that: The molar ratio of the hydrophobic monomer to the acrylamide monomer in step (2) is 1:

220.

5. The method for preparing a 3D printable ink based on dynamic hydrogel according to claim 1, characterized in that: In step (3), the cross-linking agent is N,N-methylenebisacrylamide, the initiator is ammonium persulfate, and the catalyst is tetramethylethylenediamine.

6. A 3D printable ink based on a dynamic hydrogel prepared according to the method according to any one of claims 1 to 5.

7. A use of the dynamic hydrogel-based 3D printable ink according to claim 6 in preparing transition metal sulfide three-dimensional materials, characterized in that: The method for preparing the transition metal sulfide three-dimensional material comprises the following steps: Step 1: Load the dynamic hydrogel-based 3D printable ink into a syringe and directly print to form a preset structure; Step 2: immersing the preset structure in a metal salt solution to stabilize the structure and load metal ions; Step three, freeze-drying the formed hydrogel and calcining it at high temperature to transform it to obtain a transition metal sulfide three-dimensional material.

8. The use of the dynamic hydrogel-based 3D printable ink in the preparation of transition metal sulfide three-dimensional materials according to claim 7, characterized in that: The nominal diameter of the syringe needle described in step 1 is 0.5~1.5mm, the equipment used is an extrusion 3D printing equipment, and the printing conditions are as follows: printing at room temperature; extrusion pressure is 30~40kPa; gun head moving speed: 15~20mm / s.

9. The use of the dynamic hydrogel-based 3D printable ink in the preparation of transition metal sulfide three-dimensional materials according to claim 7, characterized in that: The metal salt solution in step 2 includes one or more of ferric chloride hexahydrate, nickel sulfate heptahydrate, copper sulfate pentahydrate, tin chloride, cobalt sulfate heptahydrate, and lead nitrate, and the concentration of the metal salt solution is 0.1 to 1 mol / L.

10. The use of the dynamic hydrogel-based 3D printable ink in the preparation of transition metal sulfide three-dimensional materials according to claim 7, characterized in that: The high temperature calcination atmosphere in step 3 is an argon-hydrogen mixed gas, with the volumes of argon and hydrogen being 95% and 5% respectively; the high temperature calcination temperature is 700-900°C, the heating rate is 5-10°C / min, and then naturally cooled to room temperature.

Citation Information

Patent Citations

  • Preparation of nano-composite hydrogel ink and application of nano-composite hydrogel ink in 3D printing

    CN112795235A