Pure tungsten component and manufacturing method

Through spherical tungsten powder pasting and 3D printing technology, combined with vacuum heat treatment and stress removal annealing, the problem of insufficient high-temperature performance of tungsten and tungsten alloy components was solved, and pure tungsten components with excellent high-temperature performance and few defects were prepared.

CN116275104BActive Publication Date: 2024-11-26ADVANCED FOR MATERIALS & EQUIP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310168591.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-25
Publication Date
2024-11-26
Estimated Expiration
2043-02-25

AI Technical Summary

Technical Problem

The prior art is difficult to ensure the high-temperature performance of tungsten and tungsten alloy components, especially in the manufacturing of complex refractory metal components in the fields of aerospace, etc., and conventional methods cannot meet the high-temperature performance requirements.

Method used

Spherical tungsten powder is used as raw material to prepare pure tungsten components through powder laying and 3D printing technology. Spherical tungsten powder is a solid structure with a particle size of 20-40 microns. After vacuum heat treatment and stress removal annealing, it ensures the high-temperature performance and few defects of the components. .

Benefits of technology

The prepared pure tungsten components have excellent high-temperature performance, tensile strength between 600-700MPa, elongation rate of about 5%, high-temperature tensile strength≥500MPa, and significantly improved comprehensive mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116275104B_ABST
    Figure CN116275104B_ABST
Patent Text Reader

Abstract

The present invention provides a pure tungsten component and a manufacturing method. The method comprises: spreading spherical tungsten powder according to the designed shape of the pure tungsten component, and printing a green body of the pure tungsten component; the spherical tungsten powder is a solid structure, and the particle size is 20-40 microns; the green body of the pure tungsten component is kept at 1100-1200°C under vacuum for 3-10 hours, and cooled to obtain a pure tungsten component. In the above-mentioned manufacturing method of the pure tungsten component, spherical tungsten powder is used as a raw material for spreading powder, the spherical tungsten powder is a solid structure, there are no defects such as voids, and the spherical tungsten powder has a regular shape and a suitable particle size, which is conducive to normal spreading and stable printing. Under the action of the two aspects, the pure tungsten component obtained by the method has good high temperature performance, few defects, and excellent comprehensive mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of additive manufacturing, and in particular to a pure tungsten component and a manufacturing method thereof. Background Art

[0002] Refractory metals are widely used in aerospace and other fields due to their high melting points. For some complex refractory metal parts used under high temperature conditions, additive manufacturing technology is required. Tungsten is an important refractory metal. As the refractory metal with the highest melting point, additive manufacturing of tungsten and tungsten alloys is currently widely studied. However, in conventional methods, the high temperature performance of pure tungsten components prepared by tungsten still cannot meet the requirements. Summary of the invention

[0003] The main purpose of the present invention is to provide a pure tungsten component and a manufacturing method to solve the technical problem that it is difficult to ensure the performance of tungsten and tungsten alloy components by preparing additive powder by agglomeration of fine-grained tungsten powder.

[0004] To achieve the above object, the present invention provides a method for preparing a pure tungsten component, comprising:

[0005] Spreading spherical tungsten powder according to the designed shape of the pure tungsten component to print a green body of the pure tungsten component; the spherical tungsten powder has a solid structure and a particle size of 20-40 microns;

[0006] The green body of the pure tungsten component is kept at 1100-1200° C. under vacuum for 3-10 hours and then cooled to obtain a pure tungsten component.

[0007] Optionally, the step of keeping the green body of the pure tungsten component at 1100-1200° C. under vacuum for 3-10 hours and cooling comprises:

[0008] The green body is subjected to stress relief annealing, and then placed in a vacuum heat treatment furnace, evacuated to a vacuum degree of less than 10-3 Pa, the annealing temperature is maintained at 1200°C, the heat preservation time is 4-5h, and the green body is cooled along with the furnace.

[0009] Optionally, in the step of printing a green body of a pure tungsten component:

[0010] Fill scan power: 450W;

[0011] Filling scanning speed: 500mm / s;

[0012] Fill scan line gap: 0.05mm;

[0013] Profile scanning power: 350W;

[0014] Profile scanning speed: 600mm / s;

[0015] Number / size of checkerboard vectors: 8×8;

[0016] Checkerboard scanning power: 450W (filling power), 350W (contour scanning power);

[0017] Checkerboard scanning speed: 500mm / s (fill scanning speed), 300mm / s (contour scanning speed);

[0018] Checkerboard filling scan line gap: 0.06mm; inter-layer rotation angle: 67°.

[0019] Optionally, the method for preparing the spherical tungsten powder comprises:

[0020] Mix tungsten powder, nickel powder and iron powder and grind them to obtain mixed powder; wherein the particle size of the tungsten powder is 1-3 microns, the particle size of the nickel powder is 0.5-3 microns, and the particle size of the iron powder is 0.5-3 microns;

[0021] Granulating and pressing the mixed powder to obtain a material body;

[0022] After degreasing the material blank at 790-810° C., sintering it in a hydrogen atmosphere at 1450-1530° C. for 2-4 hours to obtain a rod;

[0023] The rod is added into a dissolving solution to remove iron and nickel in the rod, thereby obtaining the spherical tungsten powder. The dissolving solution includes an acid solution, and the acid solution can dissolve iron and nickel powders but cannot dissolve tungsten.

[0024] Optionally, the mass percentage of the tungsten powder is 93-95%, the mass percentage of the nickel powder is 3.5-5%, and the mass percentage of the iron powder is 1.5-2.1%.

[0025] Optionally, the step of granulating the mixed powder comprises: spray-drying and granulating the mixed powder at a gas temperature of 150-200°C.

[0026] Optionally, the mixed powder particles formed by granulation are pressed into a material green body under a pressure of 150-200 MPa, wherein the material green body is a sphere with a diameter of 20-50 mm or a cube with a width of 20-50 mm.

[0027] Optionally, the dissolving solution further includes hydrogen peroxide, and the acid solution is one or more of hydrochloric acid, sulfuric acid and nitric acid.

[0028] The present invention also provides a pure tungsten component obtained by the above-mentioned preparation method.

[0029] Optionally, the pure tungsten component is a special-shaped rocket shell.

[0030] In the above-mentioned manufacturing method of pure tungsten components, spherical tungsten powder is used as raw material for powder spreading. Spherical tungsten powder has a solid structure without defects such as voids. In addition, the spherical tungsten powder has a regular shape and a suitable particle size, which is conducive to normal powder spreading and stable printing. Under the effect of these two aspects, the pure tungsten components produced by this method have good high temperature performance, few defects, and excellent comprehensive mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0032] Figure 1 is a scanning electron microscope image of a rod according to an embodiment of the present application;

[0033] Figure 2 is a scanning electron microscope image of the spherical powder according to one embodiment of the present application.

[0034] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with the implementation methods and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0035] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] It should be noted that all directional indications (such as up, down, etc.) in the embodiments of the present invention are only used to explain the relative position relationship, movement status, etc. between the components under a certain specific posture (as shown in the accompanying drawings). If the specific posture changes, the directional indication will also change accordingly.

[0037] In addition, in the present invention, the descriptions such as "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" or "second" may explicitly or implicitly include at least one of the features.

[0038] Furthermore, the technical solutions between the various embodiments of the present invention may be combined with each other, but this must be based on the fact that they can be implemented by ordinary technicians in the field. When the combination of technical solutions is mutually contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0039] To achieve the above object, an embodiment of the present invention provides a method for preparing a pure tungsten component, comprising:

[0040] S10: Spreading spherical tungsten powder according to the designed shape of the pure tungsten component to print a green body of the pure tungsten component; the spherical tungsten powder is a solid structure, and the particle size is 20-40 microns.

[0041] Spherical tungsten powder is close to spherical in shape and has a particle size of 20-40 microns, so it has good powder spreading performance. Therefore, during the laser melting process, the energy of the laser beam is uniform and the performance of the tungsten component is consistent. The solid structure reduces the defects of pure tungsten components caused by voids, thereby improving the comprehensive mechanical properties of pure tungsten components.

[0042] S20: maintaining the green body of the pure tungsten component at 1100-1200° C. under vacuum for 3-10 hours, and cooling to obtain a pure tungsten component.

[0043] Optionally, the step of keeping the green body of the pure tungsten component at 1100-1200° C. under vacuum for 3-10 hours and cooling comprises:

[0044] The green body is subjected to stress relief annealing, and then placed in a vacuum heat treatment furnace, evacuated to a vacuum degree of less than 10-3 Pa, the annealing temperature is maintained at 1200°C, the heat preservation time is 4-5h, and the green body is cooled along with the furnace.

[0045] Specifically, the green body can be subjected to stress relief annealing at about 600°C, such as 590-610°C. Then, the printed green body is placed in a vacuum heat treatment furnace for high temperature treatment, and evacuated. The vacuum degree of the vacuum heat treatment furnace is less than 10-3Pa, the annealing temperature is 1100-1200°C, and the holding time is 3-10h, in order to remove hydrogen from the pure tungsten component, and then cooled with the furnace.

[0046] In the above-mentioned manufacturing method of pure tungsten components, spherical tungsten powder is used as the raw material for powder spreading. The spherical tungsten powder has a solid structure and does not have defects such as voids. Moreover, the spherical tungsten powder has a regular shape and a suitable particle size, which is conducive to normal powder spreading and stable printing. Under the action of these two aspects, the pure tungsten components produced by this method have good high-temperature performance, few defects, and excellent comprehensive mechanical properties. Specifically, the tensile strength of pure tungsten components is 600-700MPa, and the elongation is about 5%. The tensile strength of pure tungsten components is 600-700MPa, and the elongation is about 5%, which can reflect the excellent comprehensive mechanical properties. Moreover, the high-temperature tensile performance of pure tungsten components is excellent. Under the condition of 800°C, the high-temperature tensile strength is ≥500MPa.

[0047] Optionally, in the step of printing a green body of a pure tungsten component:

[0048] Fill scan power: 450W;

[0049] Filling scanning speed: 500mm / s;

[0050] Fill scan line gap: 0.05mm;

[0051] Profile scanning power: 350W;

[0052] Profile scanning speed: 600mm / s;

[0053] Number / size of checkerboard vectors: 8×8;

[0054] Checkerboard scanning power: 450W (filling power), 350W (contour scanning power);

[0055] Checkerboard scanning speed: 500mm / s (fill scanning speed), 300mm / s (contour scanning speed);

[0056] Checkerboard filling scan line gap: 0.06mm; inter-layer rotation angle: 67°.

[0057] Under this condition, SLM powder spreading 3D printing is carried out, and the printed green body has good quality.

[0058] The present invention provides a method for preparing spherical tungsten powder for additive manufacturing, comprising:

[0059] S10: ball-milling tungsten powder, nickel powder and iron powder to obtain mixed powder, wherein the particle size of the tungsten powder is 1-3 microns, the particle size of the nickel powder is 0.5-3 microns, and the particle size of the iron powder is 0.5-3 microns.

[0060] In this step, 1-3 micron tungsten powder, 0.5-3 micron nickel powder, and 0.5-3 micron iron powder can be mixed and ball-milled. During the ball-milling process, the tungsten powder, nickel powder, and iron powder are further crushed to form finer particles, and the tungsten powder, nickel powder, and iron powder are mixed more evenly. 1-3 micron tungsten powder, 0.5-3 micron nickel powder, and 0.5-3 micron iron powder are relatively easy to obtain and have low cost.

[0061] S20: granulating and pressing the mixed powder to obtain a material body.

[0062] In this step, the mixed powder is granulated to form small particles of mixed powder particles, and then pressed into shape, for example, by grinding or cold isostatic pressing, so that the mixed powder particles form a material body with a certain shape. The material body can be spherical, square, cylindrical, etc., and the specific shape is not limited. The volume of the material body is relatively small, and its maximum three-dimensional size is not too large to facilitate calcination. In some embodiments, the maximum size and minimum size of the material body in three dimensions are similar.

[0063] S30: After degreasing the material blank at 800° C., sintering it in a hydrogen atmosphere at 1450-1530° C. for 2-4 hours to obtain a rod.

[0064] The melting point of nickel powder is 212°C, the melting point of iron powder is 1538°C, and the melting point of tungsten powder is 3400°C. In this step, during the sintering process, the tungsten grains gradually grow, so the particle size of the tungsten powder gradually increases, forming a relatively regular spherical structure, that is, forming spherical tungsten powder particles.

[0065] Sintering in hydrogen atmosphere at 1450-1530℃ for 2-4 hours, the sintering degree is good, the melting point of nickel powder and iron powder is relatively low, forming a molten state, covering the surface of spherical tungsten powder particles. That is, the rod includes multiple spherical tungsten powder particles, and the adjacent spherical tungsten powder particles are filled with molten iron and nickel.

[0066] If the temperature is too high and the time is too long, a large amount of tungsten, nickel and iron may melt together, destroying the iron and nickel wrapped around the tungsten particles. The subsequent rods are not easy to break, and the tungsten particles are larger and irregular in shape. If the temperature is too low and the time is too short, the tungsten particles may not grow or may not grow to the target range.

[0067] S40: adding the rod into a dissolving solution to remove iron and nickel in the rod to obtain spherical tungsten powder, wherein the dissolving solution includes an acid solution, which can dissolve iron and nickel powders but cannot dissolve tungsten.

[0068] In this step, since the acid solution can dissolve iron and nickel powder but cannot dissolve tungsten, the iron and nickel filled between adjacent spherical tungsten powder particles are removed by the dissolving liquid, thereby obtaining spherical tungsten powder. In order to speed up the dissolution rate, in some embodiments, the rod can be broken, such as by knocking. The rod is broken to obtain a plurality of rod blocks. Then, the plurality of rod blocks are contacted with the acid solution to dissolve the iron and nickel in the rod blocks. Compared with the direct contact of the rod with the acid solution, the contact area of ​​the above method is increased, and the dissolution rate is accelerated.

[0069] In the above-mentioned method for preparing spherical tungsten powder for additive manufacturing, tungsten powder, nickel powder and iron powder are used as raw materials to sinter to obtain rods. During the sintering process, the particle size of the tungsten powder increases to form spherical tungsten powder particles with larger particles, and the nickel powder and iron powder are melted and coated on the surface of the spherical tungsten powder particles. After the nickel powder and iron powder are removed by the dissolving liquid, spherical tungsten powder is obtained. The above-mentioned method for preparing spherical tungsten powder for additive manufacturing has short steps and simple process. The obtained spherical tungsten powder has a solid particle size and a spherical powder shape, which is suitable for powder laying and stable 3D printing of additive manufacturing, and the printed parts have few defects.

[0070] In some embodiments, in the mixed powder, the mass percentage of tungsten powder is 93-95%, the mass percentage of nickel powder is 3.5-5%, and the mass percentage of iron powder is 1.5-2.1%.

[0071] In some embodiments, the material blank is degreased at 800° C. and then sintered at 1450-1530° C. in a hydrogen atmosphere for 2-4 hours to obtain a rod.

[0072] In some embodiments, in the step of ball-milling the tungsten powder, nickel powder and iron powder, the ball-milling medium is ethanol, and 1-3% paraffin is added to the ethanol. The ball-milling time is 24-36 hours, the ball-to-material ratio of the ball mill is 4:1, and the material is the sum of the tungsten powder, nickel powder and iron powder.

[0073] In some embodiments, the step of granulating the mixed powder comprises: spray drying the mixed powder at a gas temperature of 150-200° C. to granulate the mixed powder.

[0074] In some embodiments, the mixed powder particles formed by granulation are pressed into a material green body under a pressure of 150-200 MPa, and the material green body is a sphere with a diameter of 20-50 mm or a cube with a width of 20-50 mm.

[0075] In some embodiments, the dissolving solution further comprises hydrogen peroxide, and the acid solution is one or more of hydrochloric acid, sulfuric acid and nitric acid. The concentrations of the hydrochloric acid, the sulfuric acid and the nitric acid are 25-40%, and the concentration of the hydrogen peroxide is 27-50%. Exemplarily, the volume ratio of the hydrogen peroxide to the acid solution is 1:1.

[0076] In some embodiments, adding the rod to a dissolving solution to remove iron and nickel from the rod comprises:

[0077] The rod is crushed and added into the dissolving solution to dissolve, and then washed with water, neutralized and filtered to obtain the spherical tungsten powder.

[0078] Among them, water washing can remove most of the solution and the nickel ions and iron ions dissolved in the solution. There may be residual H on the surface of the tungsten particles after water washing. + , it can be removed by immersing it in an alkaline solution to neutralize its surface.

[0079] The present invention also provides spherical tungsten powder obtained by the above preparation method.

[0080] The present invention also provides an application of the spherical tungsten powder obtained by the above-mentioned preparation method in additive manufacturing of metal parts.

[0081] The present invention also provides a pure tungsten component obtained by the above-mentioned preparation method.

[0082] Optionally, the pure tungsten component is a special-shaped rocket shell.

[0083] The technical solution of the present application is described below in conjunction with specific embodiments.

[0084] Example 1

[0085] S101 ball milling: tungsten powder, nickel powder and iron powder are mixed and ball milled to obtain a mixed powder. The particle size of the tungsten powder is 3 microns, the particle size of the nickel powder is 2 microns, and the particle size of the iron powder is 3 microns. The mixed powder is 93% tungsten + 4.9% nickel + 2.1% iron powder.

[0086] S102 Spray drying: The mixed powder is dried and granulated by using a closed spray drying method with a centrifugal nozzle at a gas temperature of 150°C.

[0087] S103 pressing: Pressed by grinding or cold isostatic pressing, with a pressure of 150MPa, into small cubes with a diameter of 20mm.

[0088] S104 sintering: After degreasing the material body at 800°C, sinter it in a hydrogen atmosphere at 1500°C for 2-4 hours to obtain a rod.

[0089] S105 dissolution: dissolve the rod in hydrochloric acid and hydrogen peroxide, wash, neutralize and filter to obtain spherical tungsten powder of about 32 microns. Spherical tungsten powder has a solid structure.

[0090] S106 powder spreading and printing: SLM powder spreading 3D printing is used to 3D print the green body of the pure tungsten component according to the design shape of the pure tungsten component. The specific process parameters are:

[0091] Fill scan power: 450W;

[0092] Filling scanning speed: 500mm / s;

[0093] Fill scan line gap: 0.05mm;

[0094] Profile scanning power: 350W;

[0095] Profile scanning speed: 600mm / s;

[0096] Number / size of checkerboard vectors: 8×8;

[0097] Checkerboard scanning power: 450W (filling power), 350W (contour scanning power);

[0098] Checkerboard scanning speed: 500mm / s (fill scanning speed), 300mm / s (contour scanning speed);

[0099] Checkerboard filling scan line gap: 0.06mm; inter-layer rotation angle: 67°.

[0100] S107 high temperature heat treatment: firstly, stress relief annealing of the green body (about 600℃); then high temperature treatment, the printed green body parts are placed in a vacuum heat treatment furnace, and vacuum is drawn. The vacuum degree of the vacuum heat treatment furnace is less than 10 -3 Pa, annealing temperature 1100 ° C, holding time 3-10h, the purpose is to remove hydrogen in the pure tungsten components, and then cool with the furnace.

[0101] Example 2

[0102] S101 ball milling: tungsten powder, nickel powder and iron powder are mixed and ball milled to obtain a mixed powder. The particle size of the tungsten powder is 2 microns, the particle size of the nickel powder is 3 microns, and the particle size of the iron powder is 0.5 microns. The mixed powder is 94% tungsten + 4% nickel + 2% iron powder.

[0103] S102 Spray drying: The mixed powder is dried and granulated by using a closed spray drying method with a centrifugal nozzle at a gas temperature of 180°C.

[0104] S103 pressing: Press by grinding or cold isostatic pressing, with a pressure of 180MPa, into small balls or small cubes with a diameter of 30mm.

[0105] S104 sintering: After the material body is degreased at 800°C, it is sintered in a hydrogen atmosphere at 1450°C for 2-4 hours to obtain a rod.

[0106] S105 dissolution: dissolve the rod in nitric acid and hydrogen peroxide, wash, neutralize and filter to obtain spherical tungsten powder of about 30 microns.

[0107] S106 powder spreading and printing: SLM powder spreading 3D printing is used to 3D print the green body of the pure tungsten component according to the design shape of the pure tungsten component. The specific process parameters are:

[0108] Fill scan power: 450W;

[0109] Filling scanning speed: 500mm / s;

[0110] Fill scan line gap: 0.05mm;

[0111] Profile scanning power: 350W;

[0112] Profile scanning speed: 600mm / s;

[0113] Number / size of checkerboard vectors: 8×8;

[0114] Checkerboard scanning power: 450W (filling power), 350W (contour scanning power);

[0115] Checkerboard scanning speed: 500mm / s (fill scanning speed), 300mm / s (contour scanning speed);

[0116] Checkerboard filling scan line gap: 0.06mm; inter-layer rotation angle: 67°.

[0117] S107 high temperature heat treatment: firstly, stress relief annealing of the green body (about 600℃); then high temperature treatment, the printed green body parts are placed in a vacuum heat treatment furnace, and vacuum is drawn. The vacuum degree of the vacuum heat treatment furnace is less than 10 -3 Pa, annealing temperature 1150 ° C, holding time 6h, the purpose is to remove hydrogen in the pure tungsten components, and then cool with the furnace.

[0118] Example 3

[0119] S101 ball milling: tungsten powder, nickel powder and iron powder are mixed and ball milled to obtain a mixed powder. The particle size of the tungsten powder is 1 micron, the particle size of the nickel powder is 0.5 micron, and the particle size of the iron powder is 2 microns. The mixed powder is 95% tungsten + 3.5% nickel + 1.5% iron powder.

[0120] S102 Spray drying: The mixed powder is dried and granulated by using a closed spray drying method and a centrifugal nozzle at a gas temperature of 200°C.

[0121] S103 pressing: Press by grinding or cold isostatic pressing, with a pressure of 200MPa, into small balls or small cubes with a diameter of 20-50mm.

[0122] S104 sintering: After the material body is degreased at 800°C, it is sintered in a hydrogen atmosphere at 1530°C for 2-4 hours to obtain a rod.

[0123] S105 dissolution: dissolve the rod in sulfuric acid and hydrogen peroxide, wash, neutralize and filter to obtain spherical tungsten powder of about 35 microns.

[0124] S106 powder spreading and printing: SLM powder spreading 3D printing is used to 3D print the green body of the pure tungsten component according to the design shape of the pure tungsten component. The specific process parameters are:

[0125] Fill scan power: 450W;

[0126] Filling scanning speed: 500mm / s;

[0127] Fill scan line gap: 0.05mm;

[0128] Profile scanning power: 350W;

[0129] Profile scanning speed: 600mm / s;

[0130] Number / size of checkerboard vectors: 8×8;

[0131] Checkerboard scanning power: 450W (filling power), 350W (contour scanning power);

[0132] Checkerboard scanning speed: 500mm / s (fill scanning speed), 300mm / s (contour scanning speed);

[0133] Checkerboard filling scan line gap: 0.06mm; inter-layer rotation angle: 67°.

[0134] S107 high temperature heat treatment: firstly, stress relief annealing of the green body (about 600℃); then high temperature treatment, the printed green body parts are placed in a vacuum heat treatment furnace, and vacuum is drawn. The vacuum degree of the vacuum heat treatment furnace is less than 10 -3 Pa, annealing temperature 1200 ° C, holding time 10h, the purpose is to remove hydrogen in the pure tungsten components, and then cool with the furnace.

[0135] Comparative Example 1

[0136] The difference from Example 2 is that steps S101 to S105 are not included, and step S106 directly uses purchased tungsten powder obtained by agglomerating fine-grained tungsten powder. The remaining steps are the same as Example 1.

[0137] Comparative Example 2

[0138] The difference from Example 2 is that in step S107: first, the green body is subjected to stress relief annealing (about 600°C); then, the printed green body is subjected to high temperature treatment, and the printed green body parts are placed in a vacuum heat treatment furnace and evacuated. The vacuum degree of the vacuum heat treatment furnace is less than 10 - 3 Pa, annealing temperature 1000 ° C, holding time is 11h, and then cooled in the furnace.

[0139] Comparative Example 3

[0140] The difference from Example 3 is that in step S107: first, the green body is subjected to stress relief annealing (about 600°C); then, the printed green body parts are subjected to high temperature treatment, and the printed green body parts are placed in a vacuum heat treatment furnace and evacuated. The vacuum degree of the vacuum heat treatment furnace is less than 10- 3 Pa, annealing temperature 1300 ° C, holding time is 2h, and then cooled in the furnace.

[0141] Test Case

[0142] The rod material in step S104 of Example 1 was tested using a scanning electron microscope. The results are as follows: Figure 1 As shown. Figure 1 It can be seen that the rod includes a plurality of spherical tungsten powder particles, and the space between adjacent spherical tungsten powder particles is filled with molten iron and nickel. The shape of the spherical tungsten powder particles is relatively regular and the particle size is uniform.

[0143] The spherical tungsten powder in step S105 of Example 1 was tested using a scanning electron microscope. The results are as follows: Figure 2 As shown. Figure 2 It can be seen that the surface of the spherical tungsten powder is relatively smooth, the shape is relatively regular, and the particle size is relatively uniform, basically around 32 microns.

[0144] The pure tungsten component in step S107 of Example 1 was taken for performance testing. The tensile strength of the pure tungsten component was 603.1 MPa, and the elongation was 4.91%.

[0145] The pure tungsten component in step S107 of Example 2 was taken for performance testing. The tensile strength of the pure tungsten component was 698.5 MPa, and the elongation was 5.23%.

[0146] The pure tungsten component in step S107 of Example 3 was taken for performance testing. The tensile strength of the pure tungsten component was 662.7 MPa, and the elongation was 5.16%.

[0147] The pure tungsten component in step S107 of comparative example 1 was tested for performance. The tensile strength of the pure tungsten component was 214.2 MPa, and the elongation was 0.52%.

[0148] The pure tungsten component in step S107 of comparative example 2 was tested for performance. The tensile strength of the pure tungsten component was 286.3 MPa, and the elongation was 0.74%.

[0149] The pure tungsten component in step S107 of comparative example 3 was tested for performance. The tensile strength of the pure tungsten component was 292.8 MPa, and the elongation was 0.83%.

[0150] It can be seen that the above-mentioned method for preparing spherical tungsten powder for additive manufacturing can effectively prepare spherical tungsten powder particles with a particle size of about 30 microns. The powder shape is spherical and the particle size is relatively uniform, which is suitable for additive manufacturing powder laying and stable 3D printing.

[0151] In the above-mentioned manufacturing method of pure tungsten components, spherical tungsten powder is used as raw material for powder spreading. Spherical tungsten powder has a solid structure without defects such as voids. In addition, the spherical tungsten powder has a regular shape and a suitable particle size, which is conducive to normal powder spreading and stable printing. Under the effect of these two aspects, the pure tungsten components produced by this method have good high temperature performance, few defects, and excellent comprehensive mechanical properties.

[0152] The above technical solutions of the present invention are only preferred embodiments of the present invention, and the patent scope of the present invention is not limited thereto. All equivalent structural changes made by using the contents of the present invention specification and drawings under the technical concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A method for preparing a pure tungsten component, characterized in that: include: Spreading spherical tungsten powder according to the designed shape of the pure tungsten component to print a green body of the pure tungsten component; The spherical tungsten powder has a solid structure and a particle size of 20-40 microns; The green body is subjected to stress relief annealing, and then placed in a vacuum heat treatment furnace, and evacuated to a vacuum degree of less than 10 -3 Pa, maintain the annealing temperature at 1200°C for 4-5h, cool with the furnace to obtain a pure tungsten component; The preparation method of the spherical tungsten powder comprises: Mix tungsten powder, nickel powder and iron powder and grind them to obtain mixed powder; wherein the particle size of the tungsten powder is 1-3 microns, the particle size of the nickel powder is 0.5-3 microns, and the particle size of the iron powder is 0.5-3 microns; Granulating and pressing the mixed powder to obtain a material body; After degreasing the material blank at 790-810° C., sintering it in a hydrogen atmosphere at 1450-1530° C. for 2-4 hours to obtain a rod; The rod is added into a dissolving solution to remove iron and nickel in the rod to obtain the spherical tungsten powder, wherein the dissolving solution includes an acid solution, and the acid solution can dissolve iron and nickel powders but cannot dissolve tungsten; The ball milling medium is ethanol, and 1-3% paraffin is added to the ethanol; the ball milling time is 24-36 hours, the ball-to-material ratio of the ball milling is 4:1, and the material is the sum of the tungsten powder, the nickel powder and the iron powder; in the mixed powder, the mass percentage of the tungsten powder is 93-95%, the mass percentage of the nickel powder is 3.5-5%, and the mass percentage of the iron powder is 1.5-2.1%; The dissolving solution also includes hydrogen peroxide, and the acid solution is one or more of hydrochloric acid, sulfuric acid and nitric acid; the concentrations of the hydrochloric acid, sulfuric acid and nitric acid are 25-40%, the concentration of the hydrogen peroxide is 27-50%, and the volume ratio of the hydrogen peroxide to the acid solution is 1:

1.

2. The preparation method according to claim 1, characterized in that: In the step of printing the green body of the pure tungsten component: Fill scan power: 450W; Filling scanning speed: 500mm / s; Fill scan line gap: 0.05mm; Profile scanning power: 350W; Contour scanning speed: 600mm / s; Number / size of checkerboard vectors: 8×8; Checkerboard scanning power: filling power 450W, contour scanning power 350W; Checkerboard scanning speed: filling scanning speed 500mm / s, contour scanning speed 300mm / s; Checkerboard filling scan line gap: 0.06mm; inter-layer rotation angle: 67°.

3. The preparation method according to claim 1, characterized in that: The step of granulating the mixed powder comprises: spray drying and granulating the mixed powder at a gas temperature of 150-200°C.

4. The preparation method according to claim 3, characterized in that: The mixed powder particles formed by granulation are pressed into a material green body under a pressure of 150-200 MPa. The material green body is a sphere with a diameter of 20-50 mm or a block with a width of 20-50 mm.

5. A pure tungsten component obtained by the preparation method according to any one of claims 1 to 4.

6. The pure tungsten component according to claim 5, characterized in that: The pure tungsten component is a rocket special-shaped shell.