Cycloolefin copolymer, preparation method thereof, optical product and electronic equipment

By introducing cycloolefin copolymers with halogenated heterocyclic structures, the problem of insufficient refractive index and Abbe number in the prior art is solved, and the combination of high refractive index and low Abbe number is achieved, which satisfies high performance optics The demand for materials has expanded its application scope.

CN118978639AActive Publication Date: 2024-11-19GOERTEK OPTICAL TECH CO LTD +1

Patent Information

Application Number
CN202411036067.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-19
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

The existing cycloolefin copolymers are difficult to achieve high refractive index and low Abbe number, which limits their application in high-end optical fields, especially in the fields of high-definition imaging, such as aerospace satellites, drones and integrated circuit chip detection.

Method used

By introducing a halogenated heterocyclic structure, a cycloolefin copolymer with halogen groups is designed, and the refractive index and Abbe number are regulated through the terpolymerization method to improve the optical properties of the material.

Benefits of technology

The refractive index of cycloolefin copolymer is significantly improved to more than 1.7, meeting the needs of high-performance optical materials, while maintaining excellent light transmittance and toughness, broadening its application in the fields of optical and electronics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978639A_ABST
    Figure CN118978639A_ABST
Patent Text Reader

Abstract

The invention discloses a cycloolefin copolymer and a preparation method thereof, an optical product and electronic equipment. Wherein the cycloolefin copolymer comprises a halogenated heterocyclic structure part, and the molecular structural formula of the cycloolefin copolymer is as follows: # imgabs0 # formula (I), x, y and z are polymerization degrees and meet the conditions that x is greater than or equal to 1 and greater than or equal to 20, y is greater than or equal to 1 and z is greater than or equal to 1; m and o are the lengths of the monomer chains, 1 < = m < = 10, and 1 < = o < = 10; n is the length of the main chain, and n is more than or equal to 50 and less than or equal to 5000; and at least one of R1, R2, R3, R4, R5, R6, R7 and R8 is a halogen atom.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of cyclic olefin copolymers, and more specifically, to a cyclic olefin copolymer, a method for preparing the cyclic olefin copolymer, an optical product comprising the cyclic olefin copolymer, and an electronic device comprising the optical product. Background Art

[0002] Cyclic olefin copolymer (COC) is a new type of thermoplastic optical plastic, mainly copolymerized by cycloolefin monomers and α-olefins. In the research and development and application of optical lens materials, COC materials have become the leader in the field of optics with their unique optical properties. Especially when used as a lens material, the refractive index is related to the thinness and optical performance of the lens. In theory, the greater the refractive index of the COC material, the more significantly the thickness and weight of the lens can be reduced while maintaining the same optical performance. This is of great significance for optical equipment that pursues lightweight, portability and high imaging quality.

[0003] The refractive index of current COC materials generally hovers around 1.54, which greatly limits its application potential in high-end optical fields. In particular, in cutting-edge technology fields such as aerospace satellites, drones, and integrated circuit chip testing, the demand for ultra-clear micro lenses is growing. These fields require lens materials to have a higher refractive index to meet the precise capture of tiny details and high-definition imaging. Therefore, existing COC materials are difficult to meet these customized high-performance requirements.

[0004] In addition, the increase in the refractive index of the material is often accompanied by a problem that cannot be ignored - increased dispersion. Dispersion is the phenomenon that light is deflected to varying degrees due to different wavelengths when passing through a medium, and its degree is measured by the Abbe number (Abbe). The smaller the Abbe number, the more serious the dispersion phenomenon, which will have an adverse effect on the imaging effect of the lens, such as color distortion, blurred edges, etc. Therefore, while pursuing a high refractive index, how to effectively control and improve the Abbe number of the material to balance the relationship between the refractive index and dispersion has become a key technical problem that needs to be solved in the field of COC material research and development. Summary of the invention

[0005] One purpose of the present application is to provide a cycloolefin copolymer, which can solve the technical problems in the prior art that cycloolefin copolymers are difficult to achieve high refractive index and low Abbe number.

[0006] Another object of the present application is to provide a method for preparing a cycloolefin copolymer.

[0007] Another object of the present application is to provide an optical product prepared by the cycloolefin copolymer.

[0008] Another object of the present application is to provide an electronic device comprising the above optical product.

[0009] In order to achieve the above objectives, this application provides the following technical solutions.

[0010] According to the cyclic olefin copolymer of the first embodiment of the present application, the cyclic olefin copolymer comprises a halogenated heterocyclic structure part, and the molecular structure formula of the cyclic olefin copolymer is as follows:

[0011]

[0012] In formula (I), x, y and z are the degree of polymerization and satisfy: 20≥x≥1, y≥1, z≥1;

[0013] m, o are the lengths of the monomer chain and satisfy: 1≤m≤10, 1≤o≤10;

[0014] n is the length of the main chain and satisfies: 50≤n≤5000;

[0015] R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 and R 8 At least one of them is a halogen atom.

[0016] Optionally, in the formula (I), R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 are selected from F, Cl, Br, I, halogen atoms or H hydrogen atoms, but R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 It cannot be a H atom at the same time, and there must be at least one halogen atom.

[0017] Optionally, the R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8There are two or more halogen atoms in the

[0018] Optionally, the halogenated heterocyclic structure moiety includes a halogenated benzopyrrole, a halogenated benzodihydropyrrole or a halogenated carbazole.

[0019] Optionally, the cyclic olefin copolymer comprises the following halogenated heterocyclic polymer;

[0020]

[0021] Among them, 20≥x≥1, y≥1, z≥1, 1≤m≤10, 1≤o≤10, 50≤n≤5000.

[0022] Optionally, the cycloolefin copolymer has a high refractive index of 1.60 to 1.72;

[0023] The glass transition temperature Tg of the cycloolefin copolymer is: 200°C <Tg<300℃。

[0024] According to the preparation method of the cycloolefin copolymer of the second aspect of the present application, the preparation method comprises:

[0025] In a toluene solvent, a cycloolefin monomer, an α-olefin monomer and a halogenated heterocyclic olefin monomer are polymerized in the presence of a catalyst to obtain a cycloolefin copolymer. The molecular structure of the cycloolefin copolymer is as follows:

[0026]

[0027] In formula (I), x, y and z are the degree of polymerization and satisfy: 20≥x≥1, y≥1, z≥1;

[0028] m, o are the lengths of the monomer chain and satisfy: 1≤m≤10, 1≤o≤10;

[0029] n is the length of the main chain and satisfies: 50≤n≤5000;

[0030] R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 and R 8 At least one of them is a halogen atom.

[0031] Optionally, the structural formula of the cycloolefin monomer is as follows:

[0032]

[0033] The structural formula of the α-olefin monomer is as follows:

[0034]

[0035] The structural formula of the halogenated heterocyclic olefin monomer is as follows:

[0036]

[0037] Optionally, the halogenated heterocyclic olefin monomer is any one of the following structural formulas:

[0038]

[0039] Optionally, the catalyst is a metallocene catalyst.

[0040] Optionally, the chemical structural formula of the catalyst is any one of the following:

[0041]

[0042] Optionally, the molar ratio of the cycloolefin monomer, the α-olefin monomer and the halogenated heterocyclic olefin monomer is 1-50:1-50:5-100.

[0043] Optionally, the molar ratio of the catalyst to the cycloolefin monomer is 1:500-6000;

[0044] The molar ratio of the catalyst to the α-olefin monomer is 1:50-2000, and the α-olefin monomer is a polar or aromatic substituted olefin monomer.

[0045] Optionally, the polymerization reaction temperature is 25° C. to 150° C., and the polymerization reaction time is 0.5 h to 48 h.

[0046] According to the optical product of the third aspect of the present application, the optical product is prepared from any one of the above-mentioned cycloolefin copolymers.

[0047] The electronic device according to the fourth embodiment of the present application includes any of the above-mentioned optical products.

[0048] The beneficial effects of this application are:

[0049] The cycloolefin copolymer provided in the embodiment of the present application constructs an olefin monomer having a halogenated heterocyclic structure by introducing a halogen group with a high molar refractive index and a low molar volume into a heteroatom cyclic group. This design effectively combines two molecular structural characteristics that enhance the refractive index, so that the prepared halogenated heterocyclic olefin monomer can significantly increase the refractive index of the cycloolefin copolymer to a level greater than 1.7 after copolymerization, thereby meeting the high refractive index requirements of high-performance optical materials.

[0050] The preparation method of the cycloolefin copolymer provided in the embodiment of the present application is prepared by terpolymerization of a halogenated heterocyclic olefin monomer, an α-olefin and a cycloolefin, wherein the chain length and feed ratio of the α-olefin are adjustable, thereby regulating the glass transition temperature and elongation at break of the polymer and enhancing toughness. At the same time, the cycloolefin copolymer maintains excellent light transmittance, broadening its application in optics and related fields.

[0051] Other features and advantages of the present application will become apparent from the following detailed description of exemplary embodiments of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] Figure 1 is the H NMR spectrum of the halogenated heterocyclic monomer of Example 5 in the present application;

[0053] Figure 2 is the NMR carbon spectrum of the halogenated heterocyclic monomer of Example 5 in the present application;

[0054] Figure 3 is the H NMR spectrum of the terpolymer of Example 48 in the present application;

[0055] Figure 4 It is a comparison chart of the refractive indices of the ternary copolymers of Examples 33-42, 50, and 51 in this application;

[0056] Figure 5 is the tensile fracture curve of Example 49 in the present application;

[0057] Figure 6 This is a transmittance curve of the ternary copolymer of Example 48 in the present application. DETAILED DESCRIPTION

[0058] Various exemplary embodiments of the present application are now described in detail. It should be noted that the relative arrangement of components and steps, numerical expressions and numerical values ​​set forth in these embodiments do not limit the scope of the present application unless otherwise specifically stated.

[0059] The following description of at least one exemplary embodiment is merely illustrative in nature and is in no way intended to limit the present application, its application, or uses.

[0060] Technologies, methods, and equipment known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, the technologies, methods, and equipment should be considered part of the specification.

[0061] In all examples shown and discussed herein, any specific values ​​should be interpreted as merely exemplary and not as limiting. Therefore, other examples of the exemplary embodiments may have different values.

[0062] The cycloolefin copolymer (COC) and its preparation method, optical product and electronic device of the present application are described in detail below with reference to specific embodiments.

[0063] According to a cycloolefin copolymer provided by one embodiment of the present application, the cycloolefin copolymer comprises a halogenated heterocyclic structure portion, and the molecular structure of the cycloolefin copolymer is as follows:

[0064]

[0065] In formula (I), x, y and z are the degree of polymerization and satisfy: 20≥x≥1, y≥1, z≥1;

[0066] m, o are the lengths of the monomer chain and satisfy: 1≤m≤10, 1≤o≤10;

[0067] n is the length of the main chain and satisfies: 50≤n≤5000;

[0068] R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 and R 8 At least one of them is a halogen atom.

[0069] The cycloolefin copolymer provided in the embodiment of the present application is a high refractive index cycloolefin copolymer having a halogenated heterocycle, and the structure of the copolymer is shown in formula (I), which involves multiple variables and substituents:

[0070] x, y, z: represent the degree of polymerization of different parts, specifically 20≥x≥1, y≥1, z≥1;

[0071] m, o: represent the number of specific substituents, ranging from 1≤m≤10, 1≤o≤10 respectively;

[0072] n: represents the total degree of polymerization of the polymer, ranging from 50≤n≤5000.

[0073] Referring to formula (I), the halogenated heterocyclic structure of the cycloolefin copolymer includes R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 These eight independent substituents, and at least one of these eight independent substituents is a halogen atom.

[0074] The introduction of the halogenated heterocyclic structure not only increases the refractive index of the cycloolefin copolymer, but also enhances the chemical stability and thermal stability of the cycloolefin copolymer. This is because the bond energy between the halogen atom and the carbon atom is higher, making the material show better durability in high temperature or chemical environment.

[0075] Combined with the molecular structure of the cycloolefin copolymer, that is, formula (I), by adjusting the values ​​of x, y, z, m, o and n in formula (I), and R 1 to R 8 The specific substituents of can achieve precise control of the properties of the cycloolefin copolymer. This adjustability enables the cycloolefin copolymer to meet the special requirements of material properties in different fields.

[0076] The cycloolefin copolymer provided in the embodiment of the present application constructs an olefin monomer having a halogenated heterocyclic structure by introducing a halogen group with a high molar refractive index and a low molar volume into a heteroatom cyclic group. This design effectively combines two molecular structural characteristics that enhance the refractive index, so that the prepared halogenated heterocyclic olefin monomer can significantly increase the refractive index of the cycloolefin copolymer to a level greater than 1.7 after copolymerization, thereby meeting the high refractive index requirements of high-performance optical materials.

[0077] The cycloolefin copolymer provided in the embodiment of the present application has a high refractive index and has broad application prospects in the fields of optics, electronics, communications, etc. For example, it can be used as a high refractive index material in optical devices to improve the optical performance of the device; in electronic packaging materials, it can improve the light transmittance and thermal stability of packaging materials; in the field of communications, it can be used to make high-performance optical fibers, etc.

[0078] The cycloolefin copolymer of the embodiment of the present application is a high refractive index cycloolefin copolymer with a halogenated heterocycle. By introducing halogen atoms and halogenated heterocycle structures, the refractive index and stability of the cycloolefin copolymer material are significantly improved, and the copolymer has excellent optical properties and broad application prospects.

[0079] In some examples of the present application, the molecular structure of the cycloolefin copolymer is, that is, in formula (I), R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 are selected from F, Cl, Br, I, halogen atoms or H hydrogen atoms, but R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7, R 8 It cannot be a H atom at the same time, and there must be at least one halogen atom.

[0080] According to the description in the examples of this application, in the formula (I), R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 The eight substituents are selected from halogen atoms such as fluorine (F), chlorine (Cl), bromine (Br), iodine (I) or hydrogen (H). 1 ~R 8 ) cannot be hydrogen (H) atoms at the same time, and at least one halogen atom must be present. This design introduces specific chemical and physical properties to the cycloolefin copolymer.

[0081] About the role of halogen atoms:

[0082] The introduction of halogen atoms (especially fluorine F and chlorine Cl) can significantly affect the optical, electrical, thermal and chemical stability properties of cycloolefin copolymers. For example, the presence of halogen atoms is conducive to increasing the refractive index of cycloolefin copolymers, which is particularly important for optical materials.

[0083] Halogen atoms can also enhance the heat resistance and chemical corrosion resistance of cycloolefin copolymers, allowing them to remain stable under high temperatures or harsh chemical environments.

[0084] Regarding the restrictions on hydrogen atoms:

[0085] According to the description in the examples of this application, all substituents (i.e., R 1 ~R 8 ) cannot be hydrogen atoms at the same time, which is to ensure that the cycloolefin copolymer molecule contains at least one halogen atom, thereby giving it specific chemical and physical properties.

[0086] Due to the high polarizability of halogen atoms, their introduction may increase the refractive index of cycloolefin copolymers to greater than 1.7. In addition, the presence of halogen atoms can increase the glass transition temperature (Tg) of cycloolefin copolymers, allowing them to maintain their shape and performance at higher temperatures, which is critical for materials that need to work in high-temperature environments. In addition, the chemical inertness of halogen atoms helps to improve the resistance of cycloolefin copolymers to chemical corrosion, allowing them to maintain stable performance in a variety of chemical environments.

[0087] Due to these excellent properties, cycloolefin copolymers containing halogenated heterocyclic structures may be widely used in many fields such as optics, electronics, aerospace, and medicine.

[0088] In some examples of this application, the R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 There are two or more halogen atoms in the

[0089] In this example of the present application, it is described that R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 , R 8 There are two or more halogen atoms (such as F, Cl, Br, I) in these eight substituents. This design can bring about many technical effects:

[0090] (1) Enhance the chemical stability of cycloolefin copolymers:

[0091] The introduction of halogen atoms, especially the presence of multiple halogen atoms, can significantly improve the chemical stability of cycloolefin copolymers. Since halogen atoms have strong electronegativity, they can attract electrons and form stable covalent bonds, thereby enhancing the rigidity and stability of the molecular chain.

[0092] (2) Optimizing the physical properties of cycloolefin copolymers:

[0093] The simultaneous presence of multiple halogen atoms may also have a positive effect on the physical properties of cycloolefin copolymers. For example, the introduction of halogen atoms may change key physical parameters such as the glass transition temperature (Tg) of cycloolefin copolymers. These changes help optimize the mechanical properties and thermal stability of cycloolefin copolymers, making them more suitable for specific application scenarios.

[0094] (3) Improve and increase the optical properties of cycloolefin copolymers:

[0095] Since halogen atoms (F, Cl, Br, I) are introduced into cycloolefin copolymers, these halogen atoms have strong electronegativity and polarization ability, which can significantly increase the refractive index of the material. High refractive index materials are widely used in the optical field, such as optical lenses, optical fibers, optical guide materials, etc.

[0096] The unique electronic structure of halogen atoms may also give cycloolefin copolymers special optical properties. For example, the introduction of certain halogen atoms (such as bromine or iodine) may cause cycloolefin copolymers to absorb or emit light within a specific wavelength range, thus giving them fluorescence, phosphorescence or specific color characteristics. This improvement in optical properties has potential application value in the fields of optical materials, optoelectronic devices, etc.

[0097] In some examples of the present application, the halogenated heterocyclic structure moiety includes a halogenated benzopyrrole, a halogenated benzodihydropyrrole, or a halogenated carbazole.

[0098] The cycloolefin copolymer contains a halogenated heterocyclic structure part, which can be selected from halogenated benzopyrrole, halogenated benzodihydropyrrole or halogenated carbazole. These selections can bring at least the following effects:

[0099] The introduction of halogen atoms, especially heavy halogens such as fluorine (F), chlorine (Cl), bromine (Br) and iodine (I), can significantly increase the refractive index of cycloolefin copolymers. High refractive index is particularly important for optical materials because they can reduce the reflection loss of light at the material interface and improve optical efficiency.

[0100] The introduction of halogenated heterocycles may increase the glass transition temperature (Tg) of cycloolefin copolymers by enhancing the intermolecular interaction forces, such as the dipole-dipole interaction between halogen and neighboring atoms. A higher glass transition temperature (Tg) means that the material can maintain its physical and mechanical properties at higher temperatures, broadening the application range of the material, especially in high temperature environments.

[0101] Halogenated heterocyclic structures usually have high chemical stability and can resist corrosion from chemical reactions such as oxidation and hydrolysis. This stability enables the material to maintain its performance under harsh environmental conditions and prolongs the service life of the material.

[0102] Halogenated benzopyrrole, halogenated benzodihydropyrrole and halogenated carbazole have specific electronic structures and spectral properties, which can affect the absorption spectrum and fluorescence properties of cycloolefin copolymers. These properties are particularly important in optoelectronic devices and can achieve specific optical functions.

[0103] In some examples of the present application, the cyclic olefin copolymer includes the following halogenated heterocyclic polymer;

[0104]

[0105] Among them, 20≥x≥1, y≥1, z≥1, 1≤m≤10, 1≤o≤10, 50≤n≤5000.

[0106] According to the various halogenated heterocyclic polymers provided in the examples of this application, each halogenated heterocyclic polymer contains a halogenated heterocyclic structural part, which can be a halogenated benzopyrrole, a halogenated benzodihydropyrrole or a halogenated carbazole, etc. The introduction of these halogenated heterocycles has a significant effect on the optical, electrical or thermal properties of the cycloolefin copolymer.

[0107] The cycloolefin copolymer forms a polymer material with unique physical and chemical properties by introducing a halogenated heterocyclic structure and specific molecular structure parameters. This material has broad application prospects in the fields of optics, electronics, high temperature resistance, etc.

[0108] In some examples of the present application, the cyclic olefin copolymer has a high refractive index of 1.60 to 1.72. The glass transition temperature Tg of the cyclic olefin copolymer is: 200°C <Tg<300℃。

[0109] In the examples of this application, the cyclic olefin copolymers described exhibit two remarkable technical properties: a high refractive index and a specific glass transition temperature range.

[0110] The high refractive index (1.60-1.72) of the cycloolefin copolymer is one of its important physical properties. The refractive index is a measure of the material's ability to refract light. A high refractive index means that the material can more effectively direct light in a specific direction, which is particularly important in the application of optical materials. The application of high-refractive-index cycloolefin copolymers in optical elements can significantly improve light transmittance and focusing efficiency and reduce optical losses.

[0111] The glass transition temperature (Tg) is the temperature point at which a polymer changes from a glassy state to a highly elastic state, and is an important indicator of the thermal properties of polymer materials. In the present application, the glass transition temperature (Tg) of the cycloolefin copolymer is between 200°C and 300°C, and this temperature range is very advantageous for many practical application scenarios. A higher Tg means that the material can still maintain good shape stability and mechanical properties at high temperatures, which is especially important for optical devices that need to work at higher temperatures.

[0112] Although Tg is relatively high, it is still within the processable range, allowing molding through appropriate process conditions (such as injection molding, extrusion, etc.), making it easy to manufacture optical components with complex shapes.

[0113] When m≥1, and the value of m increases, Tg decreases significantly, while elongation at break and toughness increase. This provides the possibility of optimizing material properties by adjusting the molecular structure to meet the requirements of thermal stability and mechanical properties in different application scenarios.

[0114] Changing the values ​​of m and o at the same time can adjust the elongation at break of the cycloolefin polymer to a certain extent (≈12%), and achieve a certain degree of toughening effect.

[0115] Combining high refractive index with specific Tg range, cycloolefin copolymer in the present application has shown excellent optical properties and thermal stability. This material has a wide range of applications in the optical field, particularly in optical elements that require high light transmittance, high heat resistance and good processing properties. In addition, by adjusting the m value in the molecular structure, it is possible to balance the toughness of Tg and the material to a certain extent, further expand its application range and optimize material properties. These technical effects together make this cycloolefin copolymer become a kind of optical material with very high practical value.

[0116] According to another embodiment of the present application, a method for preparing a cycloolefin copolymer is provided, the method comprising:

[0117] In a toluene solvent, a cycloolefin monomer, an α-olefin monomer and a halogenated heterocyclic olefin monomer are polymerized in the presence of a catalyst to obtain a cycloolefin copolymer. The molecular structure of the cycloolefin copolymer is as follows:

[0118]

[0119] In formula (I), x, y and z are the degree of polymerization and satisfy: 20≥x≥1, y≥1, z≥1;

[0120] m, o are the lengths of the monomer chain and satisfy: 1≤m≤10, 1≤o≤10;

[0121] n is the length of the main chain and satisfies: 50≤n≤5000;

[0122] R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , R 7 and R 8 At least one of them is a halogen atom.

[0123] According to the preparation method of the cycloolefin copolymer provided in the embodiment of the present application, from the perspective of raw material selection, three monomers are included: cycloolefin monomer, α-olefin monomer and halogenated heterocyclic olefin monomer.

[0124] Cycloolefin monomer: As one of the main components of cycloolefin copolymer, cycloolefin monomer provides good optical properties and chemical stability. Its unique ring structure helps to form polymers with high refractive index and good heat resistance.

[0125] α-Olefin Monomer: The introduction of α-olefin can adjust the physical and chemical properties of cycloolefin copolymers, such as flexibility and processability. The performance of cycloolefin copolymers can be further optimized by changing the type and proportion of α-olefins.

[0126] Halogenated heterocyclic olefin monomers: The addition of halogenated heterocyclic olefins introduces new functional groups into cycloolefin copolymers, which may give the copolymers special reactivity, surface properties or optical properties.

[0127] The preparation method provided in the embodiment of the present application involves the use of solvents. Specifically, toluene is selected as the solvent based on its good solubility in raw materials and mildness in polymerization reaction. Toluene has a moderate boiling point, which is conducive to controlling the reaction temperature during the polymerization process and is easy to be processed subsequently, such as recovering the solvent by distillation.

[0128] Although toluene is somewhat volatile as a solvent, it is relatively easy to recycle and dispose of compared to other solvents. In addition, by optimizing the polymerization process and recycling process, the impact on the environment can be further reduced and the sustainability of production can be improved.

[0129] The preparation method provided in the embodiments of the present application involves the use of a catalyst in the polymerization process. The choice of catalyst has an important influence on the rate of polymerization, the molecular weight distribution of the product, and the structural characteristics. A suitable catalyst can ensure efficient polymerization of the monomer under mild conditions while maintaining the uniformity and stability of the product.

[0130] In the present application, by introducing different types of monomers, such as cycloolefins, α-olefins, and halogenated heterocyclic olefins, cycloolefin copolymers with complex structures and multiple properties can be prepared. This diversity provides the possibility for the application of materials in different fields.

[0131] In some examples of the present application, the structural formula of the cycloolefin monomer is as follows:

[0132]

[0133] The structural formula of the α-olefin monomer is as follows:

[0134]

[0135] The structural formula of the halogenated heterocyclic olefin monomer is as follows:

[0136]

[0137] In some examples of the present application, the halogenated heterocyclic olefin monomer is any one of the following structural formulas:

[0138]

[0139] In some examples of the present application, the catalyst is a metallocene catalyst.

[0140] The catalyst is a metallocene catalyst, which has the following technical effects:

[0141] (1) Metallocene catalysts are known for their excellent catalytic activity. In the preparation process of cycloolefin copolymers, metallocene catalysts can efficiently promote the copolymerization reaction between cycloolefin monomers, α-olefin monomers and halogenated heterocyclic olefin monomers. This high catalytic activity not only shortens the reaction time, but also improves the yield and purity of the product, thereby reducing production costs and improving production efficiency.

[0142] (2) Metallocene catalysts have excellent copolymerization ability and can precisely control the way monomers are inserted into polymer chains, thereby achieving fine control of polymer structure. In the preparation of cycloolefin copolymers, metallocene catalysts can ensure that cycloolefin monomers, α-olefin monomers, and halogenated heterocyclic olefin monomers are inserted into the polymer chain in a specific order and ratio to form copolymers with specific structures and properties. This precise control is crucial for the preparation of cycloolefin copolymers with high performance and special functions.

[0143] (3) Metallocene catalysts have high thermal and chemical stability. During the polymerization process, they can maintain activity over a wide temperature range and are not prone to decomposition or deactivation. This stability enables metallocene catalysts to adapt to different polymerization conditions, including high temperature, high pressure, and reaction systems containing specific additives. Therefore, in the preparation of cycloolefin copolymers, metallocene catalysts can ensure the smooth progress of the reaction process and improve the quality and stability of the product.

[0144] (4) Metallocene catalysts have lower toxicity and environmental pollution risks during preparation and use. They can be recycled and reused under mild conditions, thus reducing the negative impact on the environment.

[0145] In some examples of the present application, the chemical structural formula of the catalyst is any one of the following:

[0146]

[0147] In some examples of the present application, the molar ratio of the cycloolefin monomer, the α-olefin monomer and the halogenated heterocyclic olefin monomer is 1-50:1-50:5-100.

[0148] In the examples of the present application, the molar ratio of the cycloolefin monomer, the α-olefin monomer and the halogenated heterocyclic olefin monomer is set to 1-50:1-50:5-100. This ratio setting has significant technical effects in the preparation process of the cycloolefin polymer, which is mainly reflected in the following aspects:

[0149] First, the adjustability of copolymer composition;

[0150] The design of this molar ratio provides flexibility for the composition of the cycloolefin polymer. By adjusting the ratio of different monomers, the content of each type of monomer in the cycloolefin polymer can be precisely controlled, thereby regulating the physical and chemical properties of the cycloolefin polymer. For example, increasing the ratio of the halogenated heterocyclic olefin monomer may improve the heat resistance, chemical corrosion resistance or optical properties of the cycloolefin polymer.

[0151] Second, the stability of the polymerization reaction;

[0152] In copolymerization, the ratio between monomers has an impact on the stability of the polymerization reaction. Within this molar ratio range, various monomers can participate in the polymerization reaction relatively evenly, avoiding problems such as uneven reaction rate, local overheating or monomer residue caused by large differences in monomer concentration. This helps to improve the efficiency of the polymerization reaction and reduce the generation of by-products.

[0153] Third, optimization of copolymer properties;

[0154] By adjusting the monomer ratio, the properties of cycloolefin polymers can be optimized. For example, in the field of optical materials, appropriately increasing the ratio of halogenated heterocyclic olefin monomers helps to increase the refractive index of the copolymer and reduce the Abbe number.

[0155] Fourth, control of process costs

[0156] Reasonable monomer ratios also help control production costs. Under the premise of ensuring the performance of cycloolefin polymers, the amount of monomers used can be reduced by optimizing the monomer ratio, thereby reducing the cost of raw materials. At the same time, since the cycloolefin polymer reaction is more stable, the additional costs caused by uncontrolled reaction or excessive by-products are also reduced.

[0157] In some examples of the present application, the molar ratio of the catalyst to the cycloolefin monomer is 1:500-6000; the molar ratio of the catalyst to the α-olefin monomer is 1:50-2000, and the α-olefin monomer is a polar or aromatic substituted olefin monomer.

[0158] In the examples of this application, the molar ratio of the catalyst to the cycloolefin monomer and the α-olefin monomer is a key parameter in the preparation process of the cycloolefin copolymer. The molar ratio of the catalyst to the cycloolefin monomer is set to 1:500 to 1:6000, while the molar ratio to the α-olefin monomer is set to 1:50 to 1:2000. This setting has a significant technical effect on achieving efficient and controllable copolymerization and obtaining cycloolefin copolymers with excellent performance.

[0159] Specifically, the molar ratio between the catalyst and the monomer affects the reaction rate, etc. Under this setting, the amount of catalyst used is moderate relative to the monomer, which not only ensures the full effect of the catalyst, but also avoids the side reactions and cost increase that may be caused by excessive catalyst. Therefore, this ratio setting helps to achieve a higher monomer conversion rate in a shorter time and improve the overall reaction efficiency. The appropriate catalyst to monomer ratio helps to control the progress of the copolymerization reaction.

[0160] The setting of the ratio of catalyst to monomer in the present application is helpful to obtain a cycloolefin copolymer having specific performance indicators such as a refractive index and a glass transition temperature (Tg).

[0161] The cycloolefin copolymer of the present application is widely used in the fields of optics, electronics, etc. due to its unique molecular structure and excellent performance.

[0162] In some examples of the present application, the polymerization reaction temperature is 25° C. to 150° C., and the polymerization reaction time is 0.5 h to 48 h.

[0163] In the examples of this application, the setting of polymerization temperature and time (temperature is 25°C to 150°C, time is 0.5h to 48h) has a significant technical effect on the preparation process of cycloolefin copolymer. The reasonable selection of these parameters affects the polymerization rate, the molecular weight of the product and the performance of the final product.

[0164] The temperature of the polymerization reaction is one of the key factors affecting the reaction rate. Within the set temperature range (25℃~150℃), as the temperature increases, the molecular motion accelerates, and the collision frequency between the monomer and the catalyst increases, thereby accelerating the polymerization reaction. However, too high a temperature may lead to catalyst deactivation, increased side reactions, etc. Therefore, the selection of this temperature range not only ensures the reaction rate, but also avoids the occurrence of adverse factors.

[0165] At the same time, the polymerization time (0.5h to 48h) also provides fine control over the reaction process. Appropriate polymerization temperature and time are essential for obtaining cycloolefin copolymers with excellent properties. At a suitable temperature, the monomers can be inserted into the polymer chain in an orderly manner to form copolymers with regular structure and uniform molecular weight distribution. In addition, by adjusting the polymerization time, the molecular weight, crystallinity and other parameters of the copolymer can be further optimized to meet the specific requirements of material properties in different application fields.

[0166] A well-defined polymerization temperature and time range helps achieve process stability and repeatability. In production, this means that reaction conditions can be controlled more accurately, improving product consistency and quality stability.

[0167] The present application also provides an optical product, which can be prepared by the cycloolefin copolymer of any of the above embodiments. Since the cycloolefin copolymer of the embodiment of the present application achieves properties such as high refractive index and low Abbe number, the optical product of the present application also has the same advantages, which will not be described in detail here.

[0168] The present application also provides an electronic device, which includes the optical product of any of the above embodiments. Since the optical product has good optical properties, the electronic device also has the same advantages, which will not be elaborated here.

[0169] The cycloolefin copolymer according to the present application is described in detail below with reference to specific embodiments.

[0170] In the present application, the halogenated heterocyclic olefin monomer of the structural formula (IV) is preferably prepared according to the following reaction route. The halogenated heterocyclic olefin monomer is preferably norbornene. The α-olefin monomer of the structural formula (III) is preferably an α-olefin monomer.

[0171] Example 1

[0172] The preparation process of the monomer 1 having the structure of formula (IV) in this embodiment 1 is as follows:

[0173]

[0174] The specific process is as follows: 1-bromo-4-fluorobenzene (14.55 g, 0.1 mol), 2-chloro-4-fluoroaniline (17.85 g, 0.102 mol), anhydrous toluene (200 ml) and potassium tert-butoxide (13.4 g, 1.2 mol) are added to a round-bottom flask to form a mixture; the mixture is degassed and backfilled with nitrogen, and then palladium acetate (0.23 g, 0.001 mol) and tri-tert-butylphosphine tetrafluoroborate (0.435 g) are added. , 0.0015 mol), the reaction was carried out under nitrogen and stirred at 100°C for 16 h; after cooling, the mixture was treated with 1 M aqueous hydrochloric acid to neutralize, separated with water and ethyl acetate, the organic phase was collected, dried over anhydrous magnesium sulfate and filtered, the filtrate was concentrated in vacuo, and the residue was purified by silica gel chromatography with 0-20% ethyl acetate / hexane to obtain 2-chloro-4-fluoro-N-(4-fluorophenyl)aniline (17.97 g, 75%) as a light yellow oil.

[0175] Potassium carbonate (13.82 g, 0.1 mol), 2-chloro-4-fluoro-N-(4-fluorophenyl)aniline (11.98 g, 0.05 mol), tri-tert-butylphosphine tetrafluoroborate (0.217 g, 0.0075 mol), palladium acetate (0.115 g, 0.005 mol) and anhydrous N, N-dimethylacetamide (200 mL) were stirred at 110° C. for 16 h under nitrogen; after cooling, the mixture was concentrated, the residue was treated with ethyl acetate, filtered, and the filter cake was washed with ethyl acetate; the filtrate was concentrated, and the residue was purified by silica gel chromatography with 20-50% dichloromethane / n-hexane to obtain a crude product, which was recrystallized from n-hexane-dichloromethane to obtain a pure white powder product 3,6-difluorocarbazole (15.24 g, 75%).

[0176] 3,6-difluorocarbazole (20.32 g, 0.1 mol), potassium hydroxide (16.83 g, 0.3 mol), 5-bromo-1-pentene (17.88 g, 0.12 mol) and acetonitrile (250 ml) were added to a round-bottom flask, stirred and refluxed at 90°C for 12 h, and the mixture was concentrated after cooling. The residue was treated with ethyl acetate, filtered, and the filter cake was washed with ethyl acetate. The filtrate was concentrated, and the residue was purified by silica gel chromatography with 20-50% ethyl acetate / n-hexane to obtain a pure yellow-white powder target product (monomer 1) 3',6'-difluoro-5-carbazole-1-pentene (24.42 g, 90%).

[0177] 1 HNMR (400MHz, Chloroform-d) δ7.79 (dd, J=8.1, 2.8Hz, 1H), 7.63 (dd, J=7.9, 2.5Hz, 1H), 7.38 (ddd, J=8.2, 5.0, 3.4Hz, 2H), 7.07 (td, J=8.1, 2. 7Hz, 1H), 6.98 (td, J=8.0, 2.5Hz, 1H), 5.76–5.63 (m, 1H), 4.15 (t, J=6.5Hz, 2H), 2.11 (tdt, J=7.3, 5.9, 1.1Hz, 2H), 1.86 (tt, J=7.7, 6.5Hz, 2H).

[0178] Example 2

[0179] The preparation process of the monomer 2 having the structure of formula (III) in this embodiment 2 is as follows:

[0180]

[0181] The specific process is as follows: 4,4'-difluoro-2-nitro-1,1'-biphenyl (23.52 g, 0.1 mol), triphenylphosphine (65.57 g, 0.25 mol) and o-dichlorobenzene (300 ml) are added to a round-bottom flask, and heated with stirring under reflux at 175°C for 24 h; the reaction mixture is cooled to ambient temperature, and purified by column chromatography on silica gel with dichloromethane / n-hexane to obtain a yellow-white solid compound 2,7-difluorocarbazole (15.24 g, 75%).

[0182] 2,7-Difluorocarbazole (20.32 g, 0.1 mol), potassium hydroxide (16.83 g, 0.3 mol), 5-bromo-1-pentene (17.88 g, 0.12 mol) and acetonitrile (250 ml) were added to a round-bottom flask and stirred at 90°C for 12 h. After cooling, the mixture was concentrated, and the residue was treated with ethyl acetate, filtered, and the filter cake was washed with ethyl acetate; the filtrate was concentrated, and the residue was purified by silica gel chromatography with 20-50% ethyl acetate / n-hexane to obtain a pure yellow-white powder target product (monomer 2) 2',7'-difluoro-5-carbazole-1-pentene (24.42 g, 90%).

[0183] 1 HNMR (400MHz, Chloroform-d) δ8.00 (dd, J=7.9, 4.9Hz, 1H), 7.95 (dd, J=7.8, 5.0Hz, 1H), 7.17-7.07 (m, 4H), 5.76-5.63 (m, 1H) , 5.16-5.08 (m, 1H), 5.01–4.93 (m, 1H), 4.21 (t, J=6.5Hz, 2H), 2.11 (tdt, J=7.3, 5.9, 1.1Hz, 2H), 1.86 (tt, J=7.8, 6.5Hz, 2H).

[0184] Example 3

[0185] The preparation process of the monomer 3 having the structure of formula (III) in this embodiment 3 is as follows:

[0186]

[0187] The specific process is as follows: add carbazole (16.72 g, 0.1 mol), N-chloro-succinimide (29.37 g, 0.22 mol), N,N-dimethylformamide (150 mol) into a Shrek bottle, replace nitrogen several times, stir at 60°C for 2 h; extract with ethyl acetate / water, collect the organic phase and concentrate in vacuo, and purify the residue by silica gel chromatography with 20-50% ethyl acetate / n-hexane to obtain 3,6-dichlorocarbazole (20.07 g, 85%).

[0188] 3,6-dichlorocarbazole (23.61 g, 0.1 mol), potassium hydroxide (16.83 g, 0.3 mol), 5-bromo-1-pentene (17.88 g, 0.12 mol) and acetonitrile (250 ml) were added to a round-bottom flask and stirred at 90°C for 12 h. After cooling, the mixture was concentrated, the residue was treated with ethyl acetate, filtered, and the filter cake was washed with ethyl acetate; the filtrate was concentrated, and the residue was purified by silica gel chromatography with 20-50% ethyl acetate / n-hexane to obtain a pure yellow-white powder target product (monomer 3) 3',6'-difluoro-5-carbazole-1-pentene (27.37 g, 90%).

[0189] 1 HNMR (400MHz, Chloroform-d) δ7.86 (d, J=1.8Hz, 1H), 7.82 (d, J=2.5Hz, 1H), 7.47 (d, J=8.1Hz, 1H); 7.38 (d, J=8.2Hz, 1H), 7.29–7.18 (m, 2H), 5.69 (tt, J=1 7.2, 6.0Hz, 1H), 5.12 (ddt, J=17.2, 2.2, 1.0Hz, 1H), 4.97 (ddt, J=17.2, 2.2, 1 .0Hz, 1H), 4.20–4.14 (m, 2H), 2.15–2.07 (m, 2H), 1.86 (tt, J=7.7, 6.5Hz, 2H).

[0190] Example 4

[0191] The preparation process of the monomer 4 having the structure of formula (III) in this embodiment 4 is as follows:

[0192]

[0193] The specific process is as follows: 4,4'-dichloro-2-nitrobiphenyl (26.81 g, 0.1 mol), triethyl phosphite (49.84 g, 0.3 mol) and o-dichlorobenzene (200 ml) are heated at 160°C for 5 h under a nitrogen environment; after cooling, the mixture is concentrated in vacuo, and the residual liquid is separated by column chromatography on silica gel using toluene / heptane to obtain 2,7-dichlorocarbazole (1.17 g, 75%).

[0194] 2,7-Dichlorocarbazole (23.60 g, 0.1 mol), potassium hydroxide (16.83 g, 0.3 mol), 5-bromo-1-pentene (17.88 g, 0.12 mol) and acetonitrile (250 ml) were added to a round-bottom flask and stirred at 90°C for 12 h. After cooling, the mixture was concentrated, and the residue was treated with ethyl acetate, filtered, and the filter cake was washed with ethyl acetate; the filtrate was concentrated, and the residue was purified by silica gel chromatography with 20-50% ethyl acetate / n-hexane to obtain a pure yellow-white powder target product (monomer 2) 2',7'-dichloro-5-carbazole-1-pentene (27.37 g, 90%).

[0195] 1 HNMR (400MHz, Chloroform-d) δ7.99 (d, J=8.2Hz, 1H), 7.93 (d, J=7.9Hz, 1H), 7.33 (ddd, J=8.1, 6.2, 2.0Hz, 3H), 7.26 (d, J=1.8Hz, 1H), 7.20 (d, J=2.2H z, 1H), 5.69 (tt, J=17.2, 6.0Hz, 1H), 5.12 (ddt, J=17.2, 2.2, 1.0Hz, 1H), 4. 97 (ddt, J=17.2, 2.2, 1.0Hz, 1H), 2.10 (t, J=6.3Hz, 1H), 1.91–1.83 (m, 2H).

[0196] Example 5

[0197] The preparation process of the monomer 5 having the structure of formula (III) in this embodiment 5 is as follows:

[0198]

[0199] The specific process is as follows: add carbazole (16.72 g, 0.1 mol), N-bromo-succinimide (39.11 g, 0.22 mol), and N,N-dimethylformamide (150 mol) into a Shrek bottle, replace nitrogen several times, and stir at 60°C for 2 h; extract with ethyl acetate / water, collect the organic phase and concentrate in vacuo, and purify the residue by silica gel chromatography with 20-50% ethyl acetate / n-hexane to obtain 3,6-dibromocarbazole (27.62 g, 85%).

[0200] 3,6-dibromocarbazole (32.50 g, 0.1 mol), potassium hydroxide (16.83 g, 0.3 mol), 5-bromo-1-pentene (17.88 g, 0.12 mol) and acetonitrile (250 ml) were added to a round-bottom flask and stirred and refluxed at 90°C for 12 h. After cooling, the mixture was concentrated, the residue was treated with ethyl acetate, filtered, and the filter cake was washed with ethyl acetate. The filtrate was concentrated, and the residue was purified by silica gel chromatography with 20-50% ethyl acetate / n-hexane to obtain a pure yellow-white powder target product (monomer 5) 3',6'-dibromo-5-carbazole-1-pentene (35.37 g, 90%).

[0201] 1 HNMR (400MHz, Chloroform-d) δ8.06 (dd, J=2.0Hz, 1H), 7.52 (dd, J=8.7, 2.0Hz, 1H), 7.19 (d, J=8.7Hz, 1H) , 5.79 (tt, 0H), 5.05 (dd, 1H), 4.16 (t, J = 7.2Hz, 1H), 2.08 (td, J = 6.7, 6.2Hz, 1H), 1.90 (tt, J = 7.5Hz, 1H).

[0202] Example 6

[0203] The preparation process of the monomer 6 having the structure of formula (III) in this embodiment 6 is as follows:

[0204]

[0205] The specific process is as follows: 4,4'-dibromo-2-nitrobiphenyl (5.70 g, 0.1 mol), triethyl phosphite (49.84 g, 0.3 mol) and o-dichlorobenzene (200 ml) are heated at 160°C under a nitrogen environment for 5 hours; after cooling, the mixture is concentrated in vacuo, and the residual liquid is separated by column chromatography on silica gel using toluene / heptane to obtain 2,7-dibromocarbazole (243.75 g, 75%).

[0206] 2,7-Dichlorocarbazole (325.00 g, 0.1 mol), potassium hydroxide (16.83 g, 0.3 mol), 5-bromo-1-pentene (17.88 g, 0.12 mol) and acetonitrile (250 ml) were added to a round-bottom flask and stirred at 90°C for 12 h. After cooling, the mixture was concentrated, and the residue was treated with ethyl acetate and filtered with suction. The filter cake was washed with ethyl acetate; the filtrate was concentrated, and the residue was purified by silica gel chromatography with 20-50% ethyl acetate / n-hexane to obtain a pure yellow powder target product (monomer 6) 2',7'-dibromo-5-carbazole-1-pentene (35.76 g, 91%).

[0207] 1HNMR (400MHz, Chloroform-d) δ8.01 (d, J=8.0Hz, 1H), 7.97 (d, J=8.0Hz, 1H), 7.69 (d, J=1.9Hz, 1H), 7.53 (ddd, J=8.1, 4.6, 2.0Hz, 1H), 5.69 (tt, J=17.2, 6.0Hz, 1H), 5.16–4.93 (m, 1H), 4.20 (t, J=6.5Hz, 1H), 2.15–2.07 (m, 1H), 1.91–1.83 (m, 1H).

[0208] Example 7

[0209] The preparation process of the monomer 7 having the structure of formula (III) in this embodiment 7 is as follows:

[0210]

[0211] The specific process is as follows: 280 ml of acetic acid is added to a mixture of carbazole (16.72 g, 0.1 mol) and KI (21.58 g, 0.13 mol); after heating to reflux to dissolve all solids in glacial acetic acid, the mixture is cooled and ground potassium iodate (32.1 g, 0.15 mol) is added; then, the reaction mixture is heated to reflux again for 1 h and then cooled to room temperature. A large amount of compounds are precipitated during the reaction, and the crude product is separated by filtering and washing with water to obtain pure 3,6-diiodocarbazole (38.55 g, 92%) as a gray solid.

[0212] 3,6-diiodocarbazole (41.90 g, 0.1 mol), potassium hydroxide (16.83 g, 0.3 mol), 5-bromo-1-pentene (17.88 g, 0.12 mol) and acetonitrile (250 ml) were added to a round-bottom flask and stirred at 90°C for 12 h. After cooling, the mixture was concentrated, the residue was treated with ethyl acetate, filtered, and the filter cake was washed with ethyl acetate; the filtrate was concentrated, and the residue was purified by silica gel chromatography with 20-50% ethyl acetate / n-hexane to obtain a pure yellow-white powder target product (monomer 5) 3',6'-diiodo-5-carbazole-1-pentene (43.84 g, 90%).

[0213] 1HNMR (400MHz, Chloroform-d) δ8.48 (d, J=2.0Hz, 1H), 7.63 (dd, J=7.7, 2.0Hz, 1H), 7.38 (d, J=7.7Hz, 0H), 7.30 (d, J=7.7Hz, 0H), 5.69 (tt, J=17.2, 6.0Hz , 1H), 5.12 (ddt, J=17.2, 2.2, 1.0Hz, 1H), 4.97 (ddt, J=17.2, 2.2, 1.0Hz, 1H ), 4.20–4.14 (m, 1H), 2.15–2.07 (m, 1H), 1.86 (ddd, J=14.1, 7.6, 6.5Hz, 1H).

[0214] Example 8

[0215] The preparation process of the monomer 8 having the structure of formula (III) in this embodiment 8 is as follows:

[0216]

[0217] The specific process is as follows: add 4,4'-diiodo-2-nitro-1,1'-biphenyl (45.10 g, 0.1 mol), triphenylphosphine (65.57 g, 0.25 mol) and o-dichlorobenzene (300 ml) into a round-bottom flask, heat with stirring and reflux under nitrogen protection at 160°C for 16 h; cool to ambient temperature, and purify by column chromatography on silica gel with dichloromethane / n-hexane to obtain compound 2,7-diiodocarbazole (29.33 g, 70%) as a yellow solid.

[0218] 2,7-Diiodocarbazole (41.90 g, 0.1 mol), potassium hydroxide (16.83 g, 0.3 mol), 5-bromo-1-pentene (17.88 g, 0.12 mol) and acetonitrile (250 ml) were added to a round-bottom flask and stirred at 90°C for 12 h. After cooling, the mixture was concentrated, the residue was treated with ethyl acetate, filtered, and the filter cake was washed with ethyl acetate; the filtrate was concentrated, and the residue was purified by silica gel chromatography with 20-50% ethyl acetate / n-hexane to obtain a pure yellow-white powder target product (monomer 8) 2',7'-diiodo-5-carbazole-1-pentene (44.81 g, 92%).

[0219] 1HNMR (400MHz, Chloroform-d) δ8.01 (d, J=7.5Hz, 0H), 7.97 (d, J=7.5Hz, 0H), 7.73 (d, J=1.9Hz, 1H), 7.67 (dd, J=7.5, 2.0 Hz, 1H), 5.69 (tt, J=17.2, 6.0Hz, 1H), 5.24–4.91 (m, 1H), 4.20 (t, J=6.5Hz, 1H)), 2.15–2.07 (m, 1H), 1.91–1.85 (m, 1H).

[0220] Example 9-12 The preparation process of monomer 9-12 having the structure of formula (III) is as follows:

[0221]

[0222] 5-halogenoindole (5-fluoroindole 13.51 g, 5-chloroindole 15.16 g, 5-bromoindole 19.60 g or 5-iodoindole 23.41 g, 0.1 mol), potassium hydroxide (16.83 g, 0.3 mol), 5-bromo-1-pentene (17.88 g, 0.12 mol) and acetonitrile (250 ml) were added to a round-bottom flask, stirred and refluxed at 60 ° C for 8 h, cooled, concentrated the mixture, treated the residue with ethyl acetate, filtered, and the filter cake was washed with ethyl acetate; The liquid was concentrated and the residue was purified by silica gel chromatography with 20-50% ethyl acetate / n-hexane to obtain pure yellow oily liquid products (monomer 9) 5'-fluoro-5-indole-1-pentene (17.22 g, 86%), (monomer 10) 5'-chloro-5-indole-1-pentene (19.71 g, 93%), (monomer 11) 5'-bromo-5-indole-1-pentene (24.29 g, 92%), and (monomer 12) 5'-iodo-5-indole-1-pentene (28.02 g, 90%).

[0223] (Monomer 9) 5'-fluoro-5-indole-1-pentene (17.22 g, 86%), 1 HNMR (400MHz, Chloroform-d) δ7.80–7.74 (m, 1H), 7.29 (d, J=4.9Hz, 1H), 7.12 (td, J=7.9, 2.0Hz, 1H), 7.06 (d, J=7.9Hz, 0H), 6. 45–6.40 (m, 1H), 5.69 (tt, J=17.2, 6.0Hz, 1H), 5.21–4.91 (m, 2H), 4.10 (t, J=6.5Hz, 2H), 2.13–2.05 (m, 1H), 1.92–1.83 (m, 2H).

[0224] (Monomer 10) 5'-chloro-5-indole-1-pentene (19.71 g, 93%, 1 HNMR (400MHz, Chloroform-d) δ7.70–7.64 (m, 1H), 7.31–7.24 (m, 2H), 6.98 (d, J=2.2Hz, 1H), 6.45–6.40 (m, 1H), 5.69 (tt, J=17.2, 6.0Hz, 1H), 5.17–4.93 (m, 1H), 4.10 (t, J=6.5Hz, 2H), 2.24–2.02 (m, 1H), 1.98–1.75 (m, 12H).

[0225] (Monomer 11) 5'-bromo-5-indole-1-pentene (24.29 g, 92%), 1 HNMR (400MHz, Chloroform-d) δ7.91 (d, J=2.2Hz, 1H), 7.73 (s, 1H), 7.49 (s, 1H), 7.30 (s, 1H), 6.54–6.33 (m, 1H), 5.69 (tt, J=17 .2, 6.0Hz, 1H), 5.06 (dd, J=73.1, 2.4Hz, 2H), 4.10 (t, J=6.5Hz, 2H), 2.09 (dddd, J=7.4, 6.6, 5.9, 1.0Hz, 2H), 1.92–1.84 (m, 2H).

[0226] (Monomer 12) 5'-iodo-5-indole-1-pentene (28.02 g, 90%), 1 HNMR (400MHz, Chloroform-d) δ7.82–7.49 (m, 3H), 7.31 (d, J=5.1Hz, 1H), 6.44 (dd, J=5.1, 0.7Hz, 1H), 5.69 (tt, J=17 .2, 6.0Hz, 1H), 5.17–4.90 (m, 2H), 4.10 (t, J=6.5Hz, 2H), 2.09 (dddd, J=7.8, 7.0, 6.0, 1.2Hz, 2H), 1.92–1.84 (m, 2H).

[0227] Examples 13-16 The preparation process of monomers 13-16 having the structure of formula (III) is as follows:

[0228]

[0229] The specific process is as follows: add 6-halogenated indole (6-fluoroindole 13.51 g, 6-chloroindole 15.16 g, 6-bromoindole 19.60 g or 6-iodoindole 23.41 g, 0.1 mol), potassium hydroxide (16.83 g, 0.3 mol), 5-bromo-1-pentene (17.88 g, 0.12 mol) and acetonitrile (250 ml) into a round-bottom flask, and stir and reflux at 60°C for 8 h. After cooling, concentrate the mixture, treat the residue with ethyl acetate, filter it with suction, and wash the filter cake with ethyl acetate. The filtrate was concentrated and the residue was purified by silica gel chromatography with 20-50% ethyl acetate / n-hexane to obtain pure yellow oily liquid products (monomer 13) 6'-fluoro-5-indole-1-pentene (17.22 g, 86%), (monomer 14) 6'-chloro-5-indole-1-pentene (19.71 g, 93%), (monomer 15) 6'-bromo-5-indole-1-pentene (24.29 g, 92%), and (monomer 16) 6'-iodo-5-indole-1-pentene (28.02 g, 90%). (Monomer 13) 6'-Fluoro-5-indole-1-pentene (17.22 g, 86%) 1H NMR (500 MHz, Chloroform-d) δ 7.40 (dd, J = 8.0, 4.9 Hz, 1H), 7.29 (d, J = 5.0 Hz, 1H), 7.22 (dt, J = 7.8, 2.5 Hz, 1H), 6.97 (td, J = 8.1, 2.7 Hz, 1H), 6.61 (dd, J = 5.1, 2.3 Hz, 1H), 5.69 (tt, J = 17.2, 6.0 Hz, 1H), 5.22-4.83 (m, 1H), 4.08 (t, J = 6.5 Hz, 2H), 2.26-2.00 (m, 1H), 1.92-1.84 (m, 2H).

[0230] (Monomer 14) 6'-chloro-5-indole-1-pentene (19.71 g, 93%) 1 HNMR (500MHz, Chloroform-d) δ7.49 (d, J=8.3Hz, 1H), 7.47 (t, J=2.2Hz, 1H), 7.29 (d, J=5.1Hz, 1H), 7.19 (dd, J=8.2, 2.2Hz, 1H), 6.56 (dd, J=5.1, 2.3Hz, 1H), 5.69 (tt, J=17.2, 6.0Hz, 1H), 5.04 (dddt, J=73.1, 17.2, 2.2, 1.0Hz, 2H), 4.08 (t, J=6.5Hz, 2H), 2.13–2.05 (m, 2H), 1.92–1.84 (m, 2H).

[0231] (Monomer 15) 6'-bromo-5-indole-1-pentene (24.29 g, 92%) 1H NMR (500 MHz, Chloroform-d) δ 7.70 (t, J = 2.2 Hz, 1H), 7.48 (d, J = 8.3 Hz, 1H), 7.42 (dd, J = 8.4, 2.2 Hz, 1H), 7.30 (d, J = 5.1 Hz, 1H), 6.56 (dd, J = 5.1, 2.3 Hz, 1H), 5.69 (tt, J = 17.2, 6.0 Hz, 1H), 5.21-4.92 (m, 2H), 4.08 (t, J = 6.5 Hz, 2H), 2.13-2.05 (m, 2H), 1.92-1.84 (m, 2H).

[0232] (Monomer 16) 6'-iodo-5-indole-1-pentene (28.02 g, 90%) 1H NMR (500 MHz, Chloroform-d) δ 7.82 (t, J = 2.3 Hz, 1H), 7.54 (dd, J = 7.7, 2.2 Hz, 1H), 7.40 (d, J = 7.7 Hz, 1H), 7.31 (d, J = 4.9 Hz, 1H) H), 6.58 (dd, J=5.0, 2.3Hz, 1H), 5.69 (tt, J=17.2, 6.0Hz, 1H), 5.27–4.86 (m, 2H), 4.08 (t, J=6.5Hz, 2H), 2.09 (dddd, J=7.5, 6.6, 5.9, 1.0Hz, 2H), 1.92–1.84 (m, 2H).

[0233] Examples 17-20 The preparation process of monomers 17-20 having the structure of formula (III) is as follows:

[0234]

[0235] The specific process is as follows: 6-halogenated indoline (6-fluoroindoline 13.71 g, 6-chloroindole 15.36 g, 6-bromoindole 19.80 g or 6-iodoindole 23.61 g, 0.1 mol), triethylamine (30.36 g, 0.3 mol), 5-bromo-1-pentene (17.88 g, 0.12 mol) and DMF (150 ml) are added to a round-bottom flask, and stirred and refluxed at 40°C under nitrogen protection for 8 h. After cooling, the mixture is extracted with ethyl acetate / water, the organic phase is enriched, and vacuum concentrated. The residue was purified by silica gel chromatography with 20-50% ethyl acetate / n-hexane to obtain pure yellow oily liquid products (monomer 17) 6'-fluoro-5-indoline-1-pentene (17.86 g, 87%), (monomer 18) 6'-chloro-5-indoline-1-pentene (17.73 g, 89%), (monomer 19) 6'-bromo-5-indoline-1-pentene (22.71 g, 89%), (monomer 20) 6'-iodo-5-indoline-1-pentene (26.62 g, 85%).

[0236] (Monomer 17) 6'-Fluoro-5-indoline-1-pentene (17.86 g, 87%) 1 HNMR (400MHz, Chloroform-d) δ7.09 (dd, J=8.3, 5.0Hz, 1H), 6.77 (td, J=8.2, 1.9Hz, 1H), 6.52 (dd, J=8.0, 1.9Hz, 1H), 5.72 (tt, J=17.2, 7.1Hz, 1H), 5.05 (dddt, J=76.2, 1 7.0, 2.0, 1.0Hz, 1H), 3.54 (ddd, J=18.7, 5.1, 3.3Hz, 2H), 3.26 (d, J=6.8Hz, 2H), 3.0 0 (ddt, J=5.1, 3.1, 1.0Hz, 2H), 2.12–2.05 (m, 2H), 1.76 (ddd, J=8.1, 6.8, 1.3Hz, 2H).

[0237] (Monomer 18) 6'-chloro-5-indoline-1-pentene (17.73 g, 89%) 1HNMR (500MHz, Chloroform-d) δ7.13 (dt, J=8.4, 1.0Hz, 1H), 7.01 (dd, J=8.5, 1.9Hz, 1H), 6.86 (d, J=2.0Hz, 1H), 5.79–5.66 (m, 1H), 5.31–4. 83 (m, 2H), 3.54 (ddd, J=18.7, 5.1, 3.3Hz, 2H), 3.40–3.06 (m, 2H), 2.99 (ddt, J=5.3, 1.9, 0.9Hz, 2H), 2.28–1.97 (m, 2H), 1.81–1.72 (m, 2H).

[0238] (Monomer 19) 6'-bromo-5-indoline-1-pentene (22.71 g, 89%) 1 HNMR (400MHz, Chloroform-d) δ7.20 (dd, J=8.5, 1.9Hz, 1H), 7.07 (dt, J=8.5, 1.0Hz, 1H), 6.90 (d, J=2.0Hz, 1H), 5.79–5.66 (m, 1H), 5.27–4.87 (m, 2H), 3.54 (ddd, J=18.7, 5.1, 3.3Hz, 2H), 3.28–3.22 (m, 2H), 2.12–2.05 (m, 2H), 1.76 (tt, J=8.2, 6.8Hz, 2H).

[0239] (Monomer 20) 6'-iodo-5-indoline-1-pentene (26.62 g, 85%) 1 HNMR (500MHz, Chloroform-d) δ7.35 (dd, J=8.0, 1.9Hz, 1H), 7.25 (d, J=1.9Hz, 1H), 6.94 (dt, J=7.9, 1.1Hz, 1H), 5.79–5.66 (m, 1H), 5.28– 4.67 (m, 2H), 3.56 (dd, J=5.1, 3.3Hz, 2H), 3.26 (t, J=6.8Hz, 2H), 2.99 (ddd, J=4.3, 1.8, 1.1Hz, 2H), 2.12–2.05 (m, 2H), 1.81–1.72 (m, 2H).

[0240] The preparation process of monomers 21-24 having the structure of formula (III) is as follows:

[0241]

[0242] 5-halogenoindoline (5-fluoroindoline 13.71 g, 5-chloroindole 15.36 g, 5-bromoindole 19.80 g or 5-iodoindole 23.61 g, 0.1 mol), triethylamine (30.36 g, 0.3 mol), 5-bromo-1-pentene (17.88 g, 0.12 mol) and DMF (150 ml) were added to a round-bottom flask, stirred and refluxed at 40 ° C under nitrogen protection for 8 h, cooled, extracted with ethyl acetate / water, enriched organic phase, concentrated in vacuo, and the residue was The product was purified by silica gel chromatography with 20-50% ethyl acetate / n-hexane to obtain pure yellow oily liquid products (monomer 21) 5'-fluoro-5-indoline-1-pentene (17.86 g, 87%), (monomer 22) 5'-chloro-5-indoline-1-pentene (17.73 g, 89%), (monomer 23) 5'-bromo-5-indoline-1-pentene (22.71 g, 89%), and (monomer 24) 5'-iodo-5-indoline-1-pentene (26.62 g, 85%).

[0243] (Monomer 21) 5'-Fluoro-5-indoline-1-pentene (17.86 g, 87%) 1 HNMR (500MHz, Chloroform-d) δ6.87–6.86 (m, 1H), 6.86–6.84 (m, 1H), 6.78 (ddd, J=8.1, 1.8, 0.9Hz, 1H), 5.79–5.66 (m, 1H), 5.19–4.88 (m, 2H), 3.24 (t, J=6.8Hz, 2H), 2.95 (ddt, J=5.1, 3.3, 0.9Hz, 2H), 2.13–2.05 (m, 2H), 1.81–1.72 (m, 2H).

[0244] (Monomer 22) 5'-chloro-5-indoline-1-pentene (17.73 g, 89%) 1 HNMR (500MHz, Chloroform-d) δ7.04 (dd, J=8.9, 2.3Hz, 1H), 6.99 (dt, J=2.1, 1.0Hz, 1H), 6.75 (d, J=9.0Hz, 1H), 5.72 (tt, J=17.2, 7.1H z, 1H), 5.05 (dddt, J=76.2, 17.0, 2.0, 1.0Hz, 2H), 3.54 (ddd, J=18.7, 5.1, 3.3Hz, 2H), 2.09 (td, J=8.3, 7.1Hz, 2H), 1.81–1.72 (m, 2H).

[0245] (Monomer 23) 5'-bromo-5-indoline-1-pentene (22.71 g, 89%) 1HNMR (500MHz, Chloroform-d) δ7.28 (dd, J=9.0, 2.2Hz, 1H), 7.14 (dt, J=2.2, 0.9Hz, 1H), 6.71 (d, J=9.0Hz, 1H), 5.79–5.66 (m, 1H), 5.05 (dddt, J=76.2, 17.0, 2.0, 1.0Hz, 2H), 3.24 (t, J=6.8Hz, 2H), 3.01 (dddd, J=5.2, 3.1, 2.0, 1.0Hz, 2H), 2.12–2.05 (m, 2H), 1.76 (tt, J=8.2, 6.8Hz, 2H).

[0246] (Monomer 24) 5'-iodo-5-indoline-1-pentene (26.62 g, 85%) 1 HNMR (500MHz, Chloroform-d) δ7.50 (dd, J=8.5, 2.3Hz, 1H), 7.28 (dt, J=2.2, 1.0Hz, 1H), 6.62 (d, J=8.4Hz, 1H), 5.72 (tt, J=17.2, 7.1Hz, 1H), 5 .23–4.90(m, 2H), 3.54(ddd, J=18.7, 5.1, 3.3Hz, 2H), 3.24(t, J=6.8Hz, 2H), 3.00–2.98 (m, 2H), 2.19–2.00 (m, 2H), 1.76 (tt, J=8.2, 6.8Hz, 2H).

[0247] Example 25 The preparation process of monomer 25 having the structure of formula (III) is as follows:

[0248]

[0249] The specific process is: 4,4'-dibromo-2-nitrobiphenyl (35.70g, 0.1mol), triethyl phosphite (49.84g, 0.3mol) and o-dichlorobenzene (200ml) are heated at 160°C under a nitrogen environment for 5h; after cooling, vacuum concentration is performed, and the residual liquid is separated by column chromatography on silica gel with toluene / heptane to obtain 2,7-dibromocarbazole (243.75g, 75%).

[0250] Add 2,7-dibromocarbazole (32.50 g, 0.1 mol), N-bromo-succinimide (39.11 g, 0.22 mol), N,N-dimethylformamide (150 mol) into a Shrek bottle, replace nitrogen several times, stir at 60°C for 2 h; extract with ethyl acetate / water, collect the organic phase and concentrate in vacuo, and purify the residue by silica gel chromatography with 20-50% ethyl acetate / n-hexane to obtain 2,3,6,7-tetrabromocarbazole (36.20 g, 75%).

[0251] 2,3,6,7-Tetrabromocarbazole (48.28 g, 0.1 mol), potassium hydroxide (16.83 g, 0.3 mol), 5-bromo-1-pentene (17.88 g, 0.12 mol) and acetonitrile (250 ml) were added to a round-bottom flask and stirred and refluxed at 90°C for 12 h. After cooling, the mixture was concentrated, the residue was treated with ethyl acetate, filtered, and the filter cake was washed with ethyl acetate. The filtrate was concentrated, and the residue was purified by silica gel chromatography with 20-50% ethyl acetate / n-hexane to obtain a pure yellow-white powder target product (monomer 25) 2',3'6',7'-tetrabromo-5-carbazole-1-pentene (49.58 g, 90%). NMR (400MHz, Chloroform-d) δ8.08 (s, 1H), 7.97 (s, 1H), 7.41 (d, J=5.5Hz, 2H), 5.69 (tt, J=17.2, 6.0H z, 1H), 5.17–4.91 (m, 2H), 4.23–4.17 (m, 2H), 2.11 (dd, J=7.3, 1.3Hz, 2H), 1.86 (tt, J=7.7, 6.5Hz, 2H).

[0252] Example 26 The preparation process of monomer 26 having the structure of formula (III) is as follows:

[0253]

[0254] The specific process is as follows: 4,4'-diiodo-2-nitro-1,1'-biphenyl (45.10 g, 0.1 mol), triphenylphosphine (65.57 g, 0.25 mol) and o-dichlorobenzene (300 ml) were added to a round-bottom flask, and heated, stirred and refluxed at 160°C under nitrogen protection for 16 h. The mixture was cooled to ambient temperature and purified by column chromatography on silica gel using dichloromethane / n-hexane to obtain a yellow solid compound 2,7-diiodocarbazole (29.33 g, 70%).

[0255] 280 ml of acetic acid was added to a mixture of 2,7-diiodocarbazole (53.19 g, 0.1 mol) and KI (21.58 g, 0.13 mol). After heating to reflux to dissolve all solids in glacial acetic acid, the mixture was cooled and ground potassium iodate (32.1 g, 0.15 mol) was added; then, the reaction mixture was heated to reflux again for 1 h and then cooled to room temperature. A large amount of compound precipitated during the reaction, and the crude product was separated by filtration and washing with water to obtain pure 2,3,6,7-tetraiodocarbazole (70.533 g, 90%) as a gray solid.

[0256] 2,3,6,7-tetraiodocarbazole (78.37 g, 0.1 mol), potassium hydroxide (16.83 g, 0.3 mol), 5-bromo-1-pentene (17.88 g, 0.12 mol) and acetonitrile (250 ml) were added to a round-bottom flask and stirred at 90°C for 12 h. After cooling, the mixture was concentrated, the residue was treated with ethyl acetate, filtered, and the filter cake was washed with ethyl acetate. The filtrate was concentrated, and the residue was purified by silica gel chromatography with 20-50% ethyl acetate / n-hexane to obtain a pure yellow-white powder target product (monomer 8) 2',3',6',7'-tetraiodo-5-carbazole-1-pentene (43.84 g, 90%). NMR (500MHz, Chloroform-d) δ8.63 (s, 2H), 7.55 (s, 2H), 5.87–5.52 (m, 1H), 5.26–4.88 (m , 2H), 4.47–3.96 (m, 2H), 2.11 (tdt, J=7.3, 5.9, 1.1Hz, 2H), 1.86 (tt, J=7.7, 6.5Hz, 2H).

[0257] Examples 27-32 show the effects of different catalysts on the terpolymerization of heterocyclic halogenated monomers, α-olefins and cycloolefins.

[0258] First, Shrek bottle ① and bottle ② were dried in a blast drying oven at 120℃ for 1h; then, 30mL toluene, 30mmol norbornene, 15mmol 1-octene and 30mmol heterocyclic halogenated monomer 5 were added to Shrek bottle ① under nitrogen atmosphere, and then 10μmol of different metallocene catalysts (Cat.1-6) and 10mmol of dry methylaluminoxane were dissolved in 1mL toluene and added to Shrek bottle ② under nitrogen atmosphere; then the monomers in Shrek bottle ① were added to bottle ②, and then rapidly stirred (800 rpm) at 70℃ for 12h. After the reaction, the reaction solution was poured into 300ml of hydrochloric acid ethanol solution, the polymer was filtered, and the obtained polymer was repeatedly washed with acetone-ethyl acetate mixed solvent, and finally dried in a vacuum oven to constant weight. The specific reaction conditions and results are shown in Table 1.

[0259] Table 1

[0260]

[0261] It should be noted that all data are based on at least two parallel tests (unless otherwise specified). Activity: 103 gmol-1h-1. Mw is the weight average molecular weight, measured by GPC in chloroform.

[0262] It can be seen from Table 1 that the insertion rate of catalyst Cat.1 is relatively high for heterocyclic halogenated monomers.

[0263] Examples 33-40 show the effects of different heterocyclic halogenated monomers on the terpolymerization of α-olefins and cycloolefins under the preferred Cat.1 catalyst.

[0264] First, Shrek bottle ① and bottle ② were dried in a blast drying oven at 120°C for 1h; then, 30mL toluene, 30mmol norbornene, 15mmol 1-octene and 30mmol different heterocyclic halogenated monomers (monomers 2, 5, 7, 10, 11, 12, 18, 23, 25, 27) were added to Shrek bottle ① under a nitrogen atmosphere, and then 10μmol metallocene catalyst Cat.1 and 10mmol dry methylaluminoxane were dissolved in 1mL toluene and added to Shrek bottle ② under a nitrogen atmosphere; then the monomers in Shrek bottle ① were added to bottle ②, and then rapidly stirred (800 rpm) at 70°C for 12h. After the reaction, the reaction solution was poured into 300ml of hydrochloric acid ethanol solution, the polymer was filtered, and the obtained polymer was repeatedly washed with acetone-ethyl acetate mixed solvent, and finally dried in a vacuum oven to constant weight. The specific reaction conditions and results are shown in Table 2.

[0265] Table 2

[0266]

[0267] It should be noted that all data are based on the results of at least two parallel tests (unless otherwise specified). Activity: 103 gmol-1h-1. Mw is the weight average molecular weight, measured by GPC in chloroform.

[0268] It can be seen from Table 2 that when the halogenated heterocycle is a carbazole ring system, the refractive index is significantly higher than that of an indole ring system or an indoline ring system. When the number of halogen atoms on the halogenated heterocycle gradually increases, the refractive index also increases significantly.

[0269] Examples 43-51 show the effects of different ratios of monomers on the terpolymerization of heterocyclic halogenated monomers, α-olefins and cycloolefins under a preferred Cat. 1 catalyst.

[0270] First, Shrek bottle ① and bottle ② were dried in a blast drying oven at 120°C for 1h; then, 30mL toluene, and different proportions of norbornene, 1-octene and heterocyclic halogenated monomer 5 were added to Shrek bottle ① under a nitrogen atmosphere, and then 10μmol Cat.1 metallocene catalyst and 10mmol of dry methylaluminoxane were dissolved in 1mL toluene under a nitrogen atmosphere and added to Shrek bottle ②; then the monomers in Shrek bottle ① were added to bottle ②, and then rapidly stirred (800 rpm) at 70°C for 12h; after the reaction, the reaction solution was poured into 300ml of hydrochloric acid ethanol solution, the polymer was filtered, and the obtained polymer was repeatedly washed with acetone-ethyl acetate mixed solvent, and finally dried in a vacuum oven to constant weight. The specific reaction conditions and results are shown in Table 3.

[0271] Table 3

[0272]

[0273]

[0274] It should be noted that all data are based on at least two parallel tests (unless otherwise specified). Activity: 103 gmol-1h-1. Mw is the weight average molecular weight, measured by GPC in chloroform.

[0275] The data in Table 3 show that when the concentration of cycloolefin monomers is kept constant and the concentration of halogenated heterocyclic olefin monomers is increased, the insertion rate gradually increases. When the amount of 1-octene is increased, the elongation at break of the polymer increases significantly, and the glass transition temperature also decreases significantly. Compared with Mitsui 5014 products, it has obvious performance advantages in refractive index and elongation at break.

[0276] Although some specific embodiments of the present application have been described in detail by way of example, it should be understood by those skilled in the art that the above examples are only for illustration, not for limiting the scope of the present application. It should be understood by those skilled in the art that the above embodiments may be modified without departing from the scope and spirit of the present application. The scope of the present application is defined by the appended claims.

Claims

1. A cycloolefin copolymer, characterized in that: The cycloolefin copolymer comprises a halogenated heterocyclic structure portion, and the molecular structure of the cycloolefin copolymer is as follows: In formula (I), x, y and z are the degree of polymerization and satisfy: 20≥x≥1, y≥1, z≥1; m, o are the lengths of the monomer chain and satisfy: 1≤m≤10, 1≤o≤10; n is the length of the main chain and satisfies: 50≤n≤5000; At least one of R1, R2, R3, R4, R5, R6, R7 and R8 is a halogen atom.

2. The cycloolefin copolymer according to claim 1, characterized in that In the formula (Ⅰ), R1, R2, R3, R4, R5, R6, R7, R8 are selected from F, Cl, Br, I, halogen atoms or H hydrogen atoms respectively, but R1, R2, R3, R4, R5, R6, R7, R8 cannot be H atoms at the same time, and at least one halogen atom is present among them.

3. The cycloolefin copolymer according to claim 2, characterized in that There are two or more halogen atoms in R1, R2, R3, R4, R5, R6, R7 and R8.

4. The cycloolefin copolymer according to claim 1, characterized in that The halogenated heterocyclic structure moiety includes halogenated benzopyrrole, halogenated benzodihydropyrrole or halogenated carbazole.

5. The cycloolefin copolymer according to claim 1, characterized in that The cyclic olefin copolymer includes the following halogenated heterocyclic polymers; Among them, 20≥x≥1, y≥1, z≥1, 1≤m≤10, 1≤o≤10, 50≤n≤5000.

6. The cycloolefin copolymer according to claim 1, characterized in that The cyclic olefin copolymer has a high refractive index of 1.60 to 1.72; The glass transition temperature Tg of the cycloolefin copolymer is: 200°C <Tg<300℃。 7. A method for preparing a cycloolefin copolymer, characterized in that: The preparation method comprises: In a toluene solvent, a cycloolefin monomer, an α-olefin monomer and a halogenated heterocyclic olefin monomer are polymerized in the presence of a catalyst to obtain a cycloolefin copolymer. The molecular structure of the cycloolefin copolymer is as follows: In formula (I), x, y and z are the degree of polymerization and satisfy: 20≥x≥1, y≥1, z≥1; m, o are the lengths of the monomer chain and satisfy: 1≤m≤10, 1≤o≤10; n is the length of the main chain and satisfies: 50≤n≤5000; At least one of R1, R2, R3, R4, R5, R6, R7 and R8 is a halogen atom.

8. The method for preparing a cycloolefin copolymer according to claim 7, characterized in that: The structural formula of the cycloolefin monomer is as follows: The structural formula of the α-olefin monomer is as follows: The structural formula of the halogenated heterocyclic olefin monomer is as follows:

9. The method for preparing a cycloolefin copolymer according to claim 7, characterized in that: The halogenated heterocyclic olefin monomer is any one of the following structural formulas:

10. The method for preparing a cycloolefin copolymer according to claim 7, characterized in that: The catalyst is a metallocene catalyst.

11. The method for preparing a cycloolefin copolymer according to claim 10, characterized in that: The chemical structural formula of the catalyst is any one of the following:

12. The method for preparing a cycloolefin copolymer according to claim 7, characterized in that: The molar ratio of the cycloolefin monomer, the α-olefin monomer and the halogenated heterocyclic olefin monomer is 1-50:1-50:5-100.

13. The method for preparing a cycloolefin copolymer according to claim 7, characterized in that: The molar ratio of the catalyst to the cycloolefin monomer is 1:500-6000; The molar ratio of the catalyst to the α-olefin monomer is 1:50-2000, and the α-olefin monomer is a polar or aromatic substituted olefin monomer.

14. The method for preparing a cycloolefin copolymer according to claim 7, characterized in that: The polymerization reaction temperature is 25° C. to 150° C., and the polymerization reaction time is 0.5 h to 48 h.

15. An optical product, characterized in that: The optical product is prepared from the cyclic olefin copolymer according to any one of claims 1 to 6.

16. An electronic device, characterized in that: The optical product comprising claim 15.

Citation Information

Patent Citations

  • Cycloolefin copolymer and preparation method thereof

    CN115028763A

  • Cycloolefin copolymer, preparation method thereof, optical product and electronic equipment

    CN118290653A

  • Copolymerization of norbornene and functional norbornene monomers

    US20020058769A1

  • Optical film and image display apparatus having the same

    US20100272971A1

  • Process for producing polymer

    WO2006132356A1

Cited By

  • Cycloolefin copolymer, preparation method thereof and optical device

    CN121652341A