Graft-modified fluorine-containing copolymer, preparation method thereof and application of graft-modified fluorine-containing copolymer in lithium battery binder
The grafted fluorinated copolymer was prepared by graft modification, which solved the problem of insufficient adhesive performance of the binder in the existing technology, and achieved efficient improvement of adhesive performance and cost control, thereby improving the battery cycle performance and production efficiency of lithium-ion batteries.
Patent Information
- Application Number
- CN202411176257.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-19
AI Technical Summary
Existing technologies make it difficult to prepare fluorinated copolymer binders with high adhesion through simple and low-cost processes, resulting in insufficient battery cycle performance and increased costs for lithium-ion batteries.
The grafting modification method involves polymerizing a first monomer with a second monomer to form an intermediate polymer, and then modifying the intermediate polymer with a third monomer to form a grafted fluorinated copolymer. The specific steps include using vinylidene fluoride as the first monomer, a second monomer containing chlorine atoms, and a third monomer having vinyl and carboxylic acid groups, combined with an emulsifier, chain transfer agent, and initiator for polymerization.
The prepared grafted fluorinated copolymer exhibits excellent bonding properties, which improves the adhesion of electrode sheets and enhances the performance and production efficiency of lithium-ion batteries.
Smart Images

Figure CN118978642A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of polymer materials, and specifically relates to a graft-modified fluorine-containing copolymer, a preparation method of the copolymer, and application of the fluorine-containing copolymer in a lithium battery binder. Background Art
[0002] Lithium-ion batteries are increasingly widely used due to their outstanding advantages such as high specific energy, high operating voltage, light weight, low self-discharge, long cycle life, long storage life, stable discharge performance, no memory effect, and low environmental pollution. The synthesis of lithium-ion batteries requires the use of binders. For example, the electrodes of lithium-ion batteries require the use of binders to adhere the electrode active material to the current collector. The binder is often a polymer compound, and its main function is to bond and retain the active material, enhance the electronic contact between the electrode active material and the conductive agent and between the active material and the current collector, and better stabilize the structure of the electrode.
[0003] Fluoropolymers, such as polyvinylidene fluoride (PVDF), are widely used as binders in commercial lithium batteries due to their high dielectric constant, stable electrochemical window, and easy slurry formation. However, when such fluorine-containing polymers are used as binders, they have significant defects due to their own properties. For example, due to the low polarity of the PVDF molecular chain, the adhesion to the metal current collector is poor, resulting in insufficient battery cycle performance. Although increasing the amount of PVDF can improve the adhesion, it will also lead to increased costs and reduced battery capacity. Therefore, how to use a simple and low-cost process to provide a fluorine polymer binder with excellent adhesion is a common demand in the lithium battery market. As the lithium battery market continues to grow and develop worldwide, the demand for binder synthesis processes that meet the above requirements is still increasing.
[0004] In the prior art, various enterprises and scientific research institutions have invested a lot of manpower and material resources in research and development in order to overcome the above defects, but have not achieved satisfactory results. For example, the common idea is to use a suspension polymerization process and a small amount of polar comonomers, but this method has very limited improvement in bonding performance; the suspension polymerization reaction time is long and the production efficiency is low; the reactivity rate of polar comonomers and main monomers such as VDF is quite different, and the copolymerization of the two is difficult; the particle size of PVDF prepared by the suspension polymerization method is large, and the dissolution rate in NMP is very slow, which is not conducive to improving the production efficiency of battery factories.
[0005] Therefore, to date, people are still eager to develop a grafted modified fluorinated copolymer and its preparation method that can be used as a lithium battery binder. This technology should be able to synthesize a fluorinated copolymer with high adhesion in a low-cost and simple manner, which is conducive to the preparation of electrode plates with excellent performance with a small amount, thereby further improving the performance of lithium-ion batteries. Summary of the invention
[0006] The inventors of the present application have unexpectedly developed a graft-modified fluorine-containing copolymer and a preparation method and application thereof through extensive research, successfully solving the technical problems that have long been urgently needed to be solved in the prior art.
[0007] The first aspect of the present application provides a method for preparing a grafted modified fluorine-containing copolymer, the method comprising: step 1: polymerizing a first monomer and a second monomer to form an intermediate polymer; step 2: modifying the intermediate polymer with a third monomer to form the grafted fluorine-containing copolymer;
[0008] The first monomer is vinylidene fluoride;
[0009] The second monomer has a structure shown in Formula I:
[0010]
[0011] In Formula I, R 1 , R 2 , R 3 and R 4 Each independently selected from: fluorine, chlorine, hydrogen, C1-C6 alkyl optionally substituted by at least one fluorine and / or chlorine, C1-C6 alkoxy optionally substituted by at least one fluorine and / or chlorine, C2-C6 alkenyl optionally substituted by at least one fluorine and / or chlorine, provided that the second monomer contains at least one chlorine atom;
[0012] The third monomer contains at least one vinyl group and at least one group selected from a carboxylic acid group, a carboxylate group or a carboxylate group.
[0013] According to one embodiment of the first aspect of the present application, the molar ratio of the first monomer to the second monomer is 99.9:0.5 to 80:20.
[0014] According to another embodiment of the first aspect of the present application, based on 100 parts by weight of the total weight of the intermediate polymer, the amount of the third monomer is 0.1 to 20 parts by weight.
[0015] According to another embodiment of the first aspect of the present application, the second monomer is selected from one or more of the following: chlorotrifluoroethylene (CTFE), dichlorodifluoroethylene, trichloromonofluoroethylene, chlorodifluoroethylene, pentafluorochloropropylene, tetrafluorodichloropropylene, trifluorotrichloropropylene, trifluorodichloropropylene, and trifluoromonochloropropylene.
[0016] According to another embodiment of the first aspect of the present application, the third monomer is selected from one or more of the following: acrylic acid, methacrylic acid, itaconic acid, 2-(trifluoromethyl)acrylic acid, acrylate, methacrylate, itaconic acid salt, 2-(trifluoromethyl)acrylate, acrylate (C1-C12) alkyl ester, methacrylate (C1-C12) alkyl ester, itaconic acid (C1-C12) alkyl ester, 2-(trifluoromethyl)acrylate (C1-C12) alkyl ester.
[0017] According to another embodiment of the first aspect of the present application, the method uses one or more additives selected from the following: an emulsifier, a chain transfer agent, and an initiator.
[0018] According to another embodiment of the first aspect of the present application, the emulsifier is selected from one or more of the following: perfluoroalkyl ether carboxylates, perfluoroalkyl carboxylic acids, perfluoropolyether carboxylates, and perfluoroalkyl sulfonamides.
[0019] According to another embodiment of the first aspect of the present application, the chain transfer agent is selected from one or more of the following: ethyl acetate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethylene carbonate, diethyl malonate, acetone, methyl propionate, ethyl propionate, and diethyl succinate.
[0020] According to another embodiment of the first aspect of the present application, the initiator is selected from one or more of the following: diethylhexyl peroxydicarbonate, tert-butyl peroxyneodecanoate, diisopropyl peroxydicarbonate, dodecyl peroxide, dibenzoyl peroxide, tert-butyl peroxy-2-ethylhexanoate, ammonium persulfate, potassium persulfate, and sodium persulfate.
[0021] The second aspect of the present application provides a graft-modified fluorine-containing copolymer, wherein the fluorine-containing copolymer is derived from a monomer raw material comprising at least a first monomer, a second monomer and a third monomer.
[0022] The first monomer is vinylidene fluoride;
[0023] The second monomer has a structure shown in Formula I:
[0024]
[0025] In Formula I, R 1 , R 2 , R 3 and R4 Each independently selected from: fluorine, chlorine, hydrogen, C1-C6 alkyl optionally substituted by at least one fluorine and / or chlorine, C1-C6 alkoxy optionally substituted by at least one fluorine and / or chlorine, C2-C6 alkenyl optionally substituted by at least one fluorine and / or chlorine, provided that the second monomer contains at least one chlorine atom;
[0026] The third monomer contains at least one vinyl group and at least one group selected from a carboxylic acid group, a carboxylate group or a carboxylate group;
[0027] The molar ratio of the first monomer to the second monomer is 99.9:0.5 to 80:20; based on 100 parts by weight of the total weight of the first monomer and the second monomer, the amount of the third monomer is 0.1 to 20 parts by weight; the first monomer and the second monomer are at least partially contained in the main chain of the fluorine-containing copolymer, and the third monomer forms a graft connected to the main chain.
[0028] According to one embodiment of the second aspect of the present application, the graft-modified fluorine-containing copolymer is prepared by the method of the present application.
[0029] The third aspect of the present application provides a binder for a lithium battery, wherein the binder comprises a graft-modified fluorine-containing copolymer prepared by the method of the present application, or the binder comprises the graft-modified fluorine-containing copolymer of the present application.
[0030] A fourth aspect of the present application provides an electrode for a lithium battery, wherein the electrode is manufactured using the binder of the present invention.
[0031] A fifth aspect of the present application provides a lithium battery, which comprises at least two electrodes, at least one of which is manufactured using the binder of the present invention.
[0032] In the following specific implementation section, the technical solution of the present application is described in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 A flow chart showing an embodiment of a method for preparing a fluorinated copolymer according to the present application;
[0034] Figure 2 shows an infrared spectrum of an intermediate copolymer prepared according to a specific embodiment of the present application;
[0035] Figure 3 The infrared spectrum of the grafted fluorine-containing copolymer prepared according to a specific embodiment of the present application is shown. DETAILED DESCRIPTION
[0036] "Range" disclosed herein is in the form of lower limit and upper limit. It can be one or more lower limits, and one or more upper limits respectively. A given range is defined by selecting a lower limit and an upper limit. The selected lower limit and upper limit define the boundaries of a particular range. All ranges that can be defined in this way are inclusive and combinable, i.e. any lower limit can be combined with any upper limit to form a range. For example, a range of 60-120 and 80-110 is listed for a particular parameter, and it is understood that a range of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following ranges can all be expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5.
[0037] In the present invention, unless otherwise specified, the numerical range "ab" represents an abbreviation of any real number combination between a and b, where a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" have been listed in this document, and "0-5" is just an abbreviation of these numerical combinations.
[0038] In the present invention, unless otherwise specified, all embodiments and preferred embodiments mentioned herein can be combined with each other to form a new technical solution.
[0039] In the present invention, unless otherwise specified, all technical features and preferred features mentioned herein can be combined with each other to form a new technical solution.
[0040] In the present invention, unless otherwise specified, all steps mentioned herein may be performed sequentially or randomly, but are preferably performed sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order, for example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0041] In the present invention, if there is no special explanation, the "including" mentioned herein means open or closed. For example, the "including" may mean that other components not listed may also be included, or only the listed components may be included.
[0042] In the present invention, when describing the spatial relationship of a specific component or object relative to other components or objects, the terms "inside", "outside", "above", "below", etc. are used to indicate that the former is located inside, outside, above or below the latter, and the two may be in direct contact, or be separated by a certain distance or separated by a third component or object.
[0043] It should be emphasized that what is shown in the drawings and described below are only some specific embodiments of the present invention, and the protection scope of the present invention is not limited to these specific embodiments. The protection scope of the present invention is defined by the claims of the present invention, and may include any technical solution within the scope of the claims, including but not limited to further improvements and substitutions to these specific embodiments.
[0044] Figure 1 A flow chart of a method according to one embodiment of the present application is shown. Figure 1 As shown, the method comprises: step 1: polymerizing the first monomer and the second monomer to form an intermediate polymer; step 2: modifying the intermediate polymer with a third monomer to form the grafted fluorine-containing copolymer. The grafted fluorine-containing polymer is suitable for use in the preparation of batteries, more specifically, suitable for use as a binder, and is used to prepare electrodes in lithium-ion batteries, such as positive electrodes or negative electrodes.
[0045] According to one embodiment of the present application, the first monomer is vinylidene fluoride, also known as 1,1-difluoroethylene.
[0046] According to another embodiment of the present application, the second monomer has a structure shown in Formula I:
[0047]
[0048] In Formula I, R 1 , R 2 , R 3 and R 4 Each is independently selected from: fluorine, chlorine, hydrogen, C1-C6 alkyl optionally substituted by at least one fluorine and / or chlorine, C1-C6 alkoxy optionally substituted by at least one fluorine and / or chlorine, C2-C6 alkenyl optionally substituted by at least one fluorine and / or chlorine, provided that the second monomer contains at least one chlorine atom. According to an exemplary embodiment, the R 1 , R 2 , R 3 and R 4Each is independently selected from: fluorine, chlorine, hydrogen, C1-C4 alkyl optionally substituted by at least one fluorine and / or chlorine, C1-C4 alkoxy optionally substituted by at least one fluorine and / or chlorine, C2-C4 alkenyl optionally substituted by at least one fluorine and / or chlorine, provided that the second monomer contains at least one chlorine atom. According to an exemplary embodiment, the R 1 , R 2 , R 3 and R 4 Each is independently selected from: fluorine, chlorine, hydrogen, C1-C3 alkyl optionally substituted by at least one fluorine and / or chlorine, C1-C3 alkoxy optionally substituted by at least one fluorine and / or chlorine, C2-C3 alkenyl optionally substituted by at least one fluorine and / or chlorine, provided that the second monomer contains at least one chlorine atom.
[0049] According to a specific embodiment of the present application, the second monomer is selected from one or more of the following: chlorotrifluoroethylene (CTFE), dichlorodifluoroethylene, trichloromonofluoroethylene, chlorodifluoroethylene, pentafluorochloropropylene, tetrafluorodichloropropylene, trifluorotrichloropropylene, trifluorodichloropropylene, trifluoromonochloropropylene; more specifically, it can be chlorotrifluoroethylene (CTFE).
[0050] According to one embodiment of the present application, the molar ratio of the first monomer to the second monomer can be 99.9:0.5 to 80:20, for example, 99:1 to 82:18, or 98:2 to 85:15, or 96:4 to 88:12, or 95:5 to 90:10, or 94:6 to 92:8, or within the numerical range obtained by combining any two of the above end values.
[0051] According to an exemplary embodiment of the present application, in the step one, the copolymerization reaction of the first monomer and the second monomer can be carried out in various ways, such as emulsion polymerization, suspension polymerization, solution polymerization, bulk polymerization, etc.; emulsion polymerization is more preferred.
[0052] According to a specific embodiment of the present application, the copolymerization reaction of step 1 can be carried out in a reaction vessel under suitable reaction conditions with the first monomer and the second monomer. According to an exemplary embodiment of the present application, the first monomer and the second monomer are monomers in gaseous form, and the two monomers are charged into the reaction vessel as gases, and the reactor can also be additionally filled with water, an emulsifier, and other optional components; as the polymerization reaction proceeds, the first monomer and the second monomer polymerize to form an intermediate polymer, and the intermediate polymer dissolves in the water in the reactor to form an aqueous emulsion.
[0053] According to one embodiment of the present application, the amount of water added to the reactor, the first monomer and the second monomer added to the reactor, and the amount of various optional additives added to the reactor are selected so that the concentration of the aqueous emulsion formed after the reaction can be 1-50% by weight, such as 2-45% by weight, or 5-42% by weight, or 8-40% by weight, or 10-35% by weight, or 15-30% by weight, or 20-25% by weight, or within the numerical range obtained by combining any two of the above end values. The polymerization reaction of step 1 can be carried out at a temperature of 40-120°C, such as 50-100°C, or 60-90°C, or 70-80°C, or within the numerical range obtained by combining any two of the above end values.
[0054] According to one embodiment of the present application, the step 1 may use one or more of the following additives as needed: an emulsifier, a chain transfer agent, and an initiator. One or more of the additives may be added to the reactor, for example, into water.
[0055] According to one embodiment of the present application: the emulsifier is selected from one or more of the following: perfluoroalkyl ether carboxylates, perfluoroalkyl carboxylic acids, perfluoropolyether carboxylates, and perfluoroalkyl sulfonamides. According to another embodiment of the present application, based on the weight of the water in the reactor as 100 parts by weight, the amount of the emulsifier added is 0.01-1.5 parts by weight, for example, 0.05-1.2 parts by weight, or 0.1-1.0 parts by weight, or 0.2-0.8 parts by weight, or 0.3-0.7 parts by weight, or 0.4-0.5 parts by weight, or within the numerical range obtained by combining any two of the above end values.
[0056] According to one embodiment of the present application, the chain transfer agent is selected from one or more of the following: ethyl acetate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethylene carbonate, diethyl malonate, acetone, methyl propionate, ethyl propionate, diethyl succinate. According to another embodiment of the present application, based on the weight of the water in the reactor as 100 parts by weight, the content of the chain transfer agent is 0.003-5 parts by weight, for example, 0.005-4.5 parts by weight, or 0.01-4.0 parts by weight, or 0.05-3.5 parts by weight, or 0.1-3.0 parts by weight, or 0.2-2.5 parts by weight, or 0.5-2.0 parts by weight, or 0.8-1.5 parts by weight, or 1.0-1.2 parts by weight, or within the numerical range obtained by combining any two of the above end values.
[0057] According to one embodiment of the present application, the initiator is selected from one or more of the following: diethylhexyl peroxydicarbonate, tert-butyl peroxyneodecanoate, diisopropyl peroxydicarbonate, dodecyl peroxide, dibenzoyl peroxide, tert-butyl peroxy-2-ethylhexanoate, ammonium persulfate, potassium persulfate, sodium persulfate. According to another embodiment of the present application, based on the weight of the water in the reactor as 100 parts by weight, the content of the initiator is 0.05-5.0 parts by weight, for example, 0.08-4.5 parts by weight, or 0.10-4.0 parts by weight, or 0.15-3.5 parts by weight, or 0.50-3.0 parts by weight, or 0.80-2.5 parts by weight, or 1.0-2.0 parts by weight, or 1.2-1.8 parts by weight, or 1.4-1.5 parts by weight, or within the numerical range obtained by combining any two of the above end values.
[0058] According to one embodiment of the present application, the polymer emulsion prepared in step 1 can be dried, washed, and other steps to obtain an intermediate polymer.
[0059] According to one embodiment of the present application, the polydispersity (also known as molecular weight distribution, Mw / Mn) of the grafted fluorinated copolymer prepared by the present invention can be 1.5-3.5, for example, 1.8-3.2, or 2.0-3.0, or 2.2-2.8, or 2.3-2.7, or within the numerical range obtained by combining any two of the above end values.
[0060] According to one embodiment of the present application, the first monomer and the second monomer form an intermediate polymer, the main chain of the intermediate polymer comprises copolymer units derived from the first monomer and the second monomer, wherein the copolymer unit derived from the second monomer comprises at least one chlorine atom, and in the subsequent step two, the copolymer unit derived from the second monomer reacts with the third monomer by means of the chlorine atom thereon, so that the third monomer, the residue derived from the third monomer, or the polymerized graft structure derived from the third monomer is connected to the main chain of the intermediate polymer (preferably forming a graft structure), thereby forming a final grafted fluorinated copolymer.
[0061] According to one embodiment of the present application, the third monomer contains at least one vinyl group and at least one group selected from a carboxylic acid group, a carboxylate group or a carboxylate group. For example, the third monomer can be selected from one or more of the following: acrylic acid, methacrylic acid, itaconic acid, 2-(trifluoromethyl) acrylic acid, acrylate, methacrylate, itaconate, 2-(trifluoromethyl) acrylic acid, acrylic acid (C1-C12) alkyl ester, methacrylate (C1-C12) alkyl ester, itaconate (C1-C12) alkyl ester, 2-(trifluoromethyl) acrylic acid (C1-C12) alkyl ester; for example, it can be selected from one or more of the following: acrylic acid, methacrylic acid, itaconic acid, 2-(trifluoromethyl) acrylic acid, acrylate, methacrylate, itaconate, 2-(trifluoromethyl) acrylic acid, acrylic acid (C1-C6) alkyl ester, methacrylate (C1-C6) alkyl ester, itaconate (C1-C6) alkyl ester, 2-(trifluoromethyl) acrylic acid (C1-C6) alkyl ester. According to a specific embodiment of the present application, the third monomer is selected from one or more of the following: 2-(trifluoromethyl)acrylic acid, acrylic acid, and methacrylic acid.
[0062] According to one embodiment of the present application, based on 100 parts by weight of the total amount of the first monomer and the second monomer, the amount of the third monomer is 0.1-20 parts by weight, for example, 0.5-18 parts by weight, or 1-16 parts by weight, or 2-15 parts by weight, or 5-12 parts by weight, or 6-10 parts by weight, or 8-9 parts by weight, or within the numerical range obtained by combining any two of the above end values.
[0063] According to one embodiment of the present application, the step 2 can be carried out under suitable conditions. For example, the polymerization temperature of the step 2 can be 60-180°C, or 70-160°C, or 80-140°C, or 90-130°C, or 100-120°C, or within the numerical range obtained by combining any two of the above end values.
[0064] In the step 2, various solvents, catalysts and additives can be used as needed. Examples of solvents include DMSO; examples of catalysts include organic metal complexes, such as copper-bipyridine complexes.
[0065] According to one embodiment of the present application, the weight average molecular weight (Mw) of the grafted fluorinated copolymer prepared by the present invention can be 2,000 to 5,000,000, for example, 3,000 to 4,000,000, or 4,000 to 3,000,000, or 5,000 to 2,000,000, or 10,000-1,800,000, or 239196
[0066] 100,000-1,500,000, or 500,000-1,200,000, or 800,000-1,100,000, or 900,000-1,000,000, or within a numerical range obtained by combining any two of the above end values.
[0067] According to a specific embodiment of the present application, in the grafted fluorine-containing copolymer of the present application, its polymeric main chain is mainly formed by the first monomer and the second monomer, and the third monomer forms a grafted structure grafted on the polymeric main chain. According to an embodiment of the present application, 80 mol% of the main chain of the grafted fluorine-containing copolymer is formed by the first monomer and the second monomer, for example, 85 mol% of the main chain is formed by the first monomer and the second monomer, or 90 mol% of the main chain is formed by the first monomer and the second monomer, or 92 mol% of the main chain is formed by the first monomer and the second monomer, or 95 mol% of the main chain is formed by the first monomer and the second monomer, or 98 mol% of the main chain is formed by the first monomer and the second monomer, or 99 mol% of the main chain is formed by the first monomer and the second monomer, or 99.9 mol% of the main chain is formed by the first monomer and the second monomer, or 100 mol% of the main chain is formed by the first monomer and the second monomer.
[0068] According to a specific embodiment of the present application, the method of the present invention comprises the following steps: (1) adding deionized water and an emulsifier into a reactor, stirring evenly and evacuating at room temperature, and then replacing the oxygen content in the reactor with nitrogen until the oxygen content is less than 50 ppm; (2) heating the reactor to 70-90°C, introducing the first monomer and the second monomer in gaseous state, so that the pressure in the reactor rises to 2.5-4.5 MPa, injecting a chain transfer agent and an initiator into the reactor through a metering pump to initiate the reaction, terminating the reaction, cooling and releasing the pressure to remove the remaining gas, then releasing the slurry and washing until the wastewater conductivity is reduced to less than 2 μs / cm, and drying to obtain an intermediate polymer; (3) using the intermediate polymer as a raw material, under the action of a catalyst, polymerizing the third monomer to form a graft connected to the main chain to obtain a final graft copolymer.
[0069] According to one embodiment of the present application, the grafted fluorine-containing copolymer of the present application can be used as a binder for preparing electrodes in lithium-ion batteries, and exhibits extremely excellent bonding properties, such as excellent bonding between the slurry (such as the slurry used to form the positive electrode active layer or the negative electrode active layer) and the current collector.
[0070] Example
[0071] The preferred embodiments of the present invention are specifically listed in the following examples, but it should be understood that the protection scope of the present application is not limited thereto. Any equivalent changes or modifications made according to the essence of the present application should be included in the protection scope of the present application.
[0072] Example 1
[0073] (i) Preparation of P(VDF-CTFE) copolymer:
[0074] In a 25-liter high-pressure polymerization reactor equipped with a stirrer, 15 kg of deionized water and 15 g of CF 3 CF 2 CF 2 O(CF(CF 3 )CF 2 O)CF(CF 3 )COONa. Close the reactor, start stirring, evacuate the reactor and replace the atmosphere with nitrogen until the oxygen content of the atmosphere in the reactor is less than 50ppm. At this time, the temperature of the reactor is raised to 80°C, and VDF / CTFE mixed monomers are charged into the reactor through a membrane pump until the pressure in the reactor is 3.5MPa. The molar content of VDF in the gaseous monomer mixture is 95 mol%. 4.6 grams of ethyl acetate and 15 grams of potassium persulfate (made into an aqueous solution) are pumped into the reactor in sequence through a metering pump to initiate polymerization. During the entire polymerization process, VDF / CTFE mixed monomers are continuously charged through a pressure automatic control system to maintain a constant pressure in the reactor at 3.5MPa. The VDF / CTFE monomer mixed gas feed rate is set to 3.5 kg. When the monomer consumption reaches 25%, 5 grams of potassium persulfate (made into an aqueous solution) are added to the reactor. When the monomer consumption reaches 50%, 5 grams of potassium persulfate (made into an aqueous solution) are added again. When the specified weight of the mixed gas is added, the feeding is stopped, and the total reaction time is 2.4 hours. After the reaction is completed, the temperature is lowered to room temperature and the pressure is released, and the obtained emulsion is coagulated and washed until the wastewater conductivity is less than 2μs / cm. The concentrated polymer slurry is spray-dried to obtain a product of white powder. Figure 2 The infrared spectrum of the white powder product is shown, from which it can be seen that the above first polymerization reaction forms a copolymer of VDF and CTFE.
[0075] (ii) Preparation of P(VDF-CTFE)-g-4PAA graft copolymer:
[0076] 200 g of the P(VDF-CTFE) copolymer obtained in step (i) was added to a three-necked flask, 500 mL of DMSO was added to the three-necked flask, and the mixture was stirred vigorously at 100 ° C until completely dissolved, and the atmosphere in the three-necked flask was replaced with nitrogen. 6.5 g of copper powder, 18 g of 4,4-bipyridine and 4 g of acrylic acid (abbreviated as AA) were added to the solution under a nitrogen atmosphere. The three-necked flask was sealed and the stirring reaction was continued for 4 hours. After the reaction was completed, the temperature of the three-necked flask was brought to room temperature, and the reaction solution was poured into 1 liter of water to precipitate the reaction product. The collected precipitate was dissolved in DMF and precipitated in water several times to remove impurities. The final polymer product was recorded as P(VDF-CTFE)-g-4PAA. Figure 3 The infrared spectrum of the polymerization product is shown. From the infrared spectrum, it can be seen that the second step polymerization reaction forms a copolymer having a VDF-CTFE main chain and a PAA graft connected to the main chain.
[0077] Example 2
[0078] (i) Preparation of P(VDF-CTFE) copolymer:
[0079] In a 25-liter high-pressure polymerization reactor equipped with a stirrer, 15 kg of deionized water and 15 g of CF 3 CF 2 CF 2 O(CF(CF 3 )CF 2 O)CF(CF 3 )COONa. Close the reactor, start stirring, evacuate the reactor and replace the atmosphere with nitrogen until the oxygen content of the atmosphere in the reactor is less than 50ppm. At this time, the temperature of the reactor is raised to 80°C, and VDF / CTFE mixed monomers are charged into the reactor through a membrane pump until the pressure in the reactor is 3.5MPa. The molar content of VDF in the gaseous monomer mixture is 90 mol%. 4.6 grams of ethyl acetate and 15 grams of potassium persulfate (made into an aqueous solution) are pumped into the reactor in sequence through a metering pump to initiate polymerization. During the entire polymerization process, VDF / CTFE mixed monomers are continuously charged through a pressure automatic control system to maintain a constant pressure in the reactor at 3.5MPa. The VDF / CTFE monomer mixed gas feed rate is set to 3.5 kg. When the monomer consumption reaches 25%, 5 grams of potassium persulfate (made into an aqueous solution) are added to the reactor. When the monomer consumption reaches 50%, 5 grams of potassium persulfate (made into an aqueous solution) are added again. When the specified weight of the mixed gas is added, the feeding is stopped, and the total reaction time is 2.6 hours. After the reaction is completed, the temperature is lowered to room temperature and the pressure is released, and the obtained emulsion is coagulated and washed until the wastewater conductivity is less than 2μs / cm. The concentrated polymer slurry is spray-dried to obtain a product of white powder.
[0080] (ii) Preparation of P(VDF-CTFE)-g-8PAA graft copolymer:
[0081] 200 g of the P(VDF-CTFE) copolymer obtained in step (i) was added to a three-necked flask, 500 mL of DMSO was added to the three-necked flask, and the mixture was stirred vigorously at 100 ° C until completely dissolved, and the atmosphere in the three-necked flask was replaced with nitrogen. 6.5 g of copper powder, 18 g of 4,4-bipyridine and 8 g of acrylic acid (abbreviated as AA) were added to the solution under a nitrogen atmosphere. The three-necked flask was sealed and the stirring reaction was continued for 4 hours. After the reaction was completed, the temperature of the three-necked flask was brought to room temperature, and the reaction solution was poured into 1 liter of water to precipitate the reaction product. The collected precipitate was dissolved in DMF and precipitated in water several times to remove impurities. The final polymer product was recorded as P(VDF-CTFE)-g-8PAA.
[0082] Example 3
[0083] (i) Preparation of P(VDF-CTFE) copolymer:
[0084] In a 25-liter high-pressure polymerization reactor equipped with a stirrer, 15 kg of deionized water and 15 g of CF 3 CF 2 CF 2 O(CF(CF 3 )CF 2 O)CF(CF 3 )COONa. Close the reactor, start stirring, evacuate the reactor and replace the atmosphere with nitrogen until the oxygen content of the atmosphere in the reactor is less than 50ppm. At this time, the temperature of the reactor is raised to 80°C, and VDF / CTFE mixed monomers are charged into the reactor through a membrane pump until the pressure in the reactor is 3.5MPa. The molar content of VDF in the gaseous monomer mixture is 95 mol%. 4.6 grams of ethyl acetate and 15 grams of potassium persulfate (made into an aqueous solution) are pumped into the reactor in sequence through a metering pump to initiate polymerization. During the entire polymerization process, VDF / CTFE mixed monomers are continuously charged through a pressure automatic control system to maintain a constant pressure in the reactor at 3.5MPa. The VDF / CTFE monomer mixed gas feed rate is set to 3.5 kg. When the monomer consumption reaches 25%, 5 grams of potassium persulfate (made into an aqueous solution) are added to the reactor. When the monomer consumption reaches 50%, 5 grams of potassium persulfate (made into an aqueous solution) are added again. When the specified weight of the mixed gas is added, the feeding is stopped, and the total reaction time is 2.3 hours. After the reaction is completed, the temperature is lowered to room temperature and the pressure is released, and the obtained emulsion is coagulated and washed until the wastewater conductivity is less than 2μs / cm. The concentrated polymer slurry is spray-dried to obtain a product of white powder.
[0085] (ii) Preparation of P(VDF-CTFE)-g-4PTFAA graft copolymer:
[0086] 200 grams of the P(VDF-CTFE) copolymer obtained in step (i) was added to a three-necked flask, 500 mL of DMSO was added to the three-necked flask, and the mixture was stirred vigorously at 100 ° C until completely dissolved, and the atmosphere in the three-necked flask was replaced with nitrogen. 6.5 grams of copper powder, 18 grams of 4,4-bipyridine and 4 grams of 2-(trifluoromethyl)acrylic acid (abbreviated as TFAA) were added to the solution under a nitrogen atmosphere. The three-necked flask was closed and the stirring reaction was continued for 4 hours. After the reaction was completed, the temperature of the three-necked flask was brought to room temperature, and the reaction solution was poured into 1 liter of water to precipitate the reaction product. The collected precipitate was dissolved in DMF and precipitated in water several times to remove impurities. The final polymer product was recorded as P(VDF-CTFE)-g-4PTFAA.
[0087] Comparative Example 1
[0088] Preparation of PVDF homopolymer:
[0089] In a 25-liter high-pressure polymerization reactor equipped with a stirrer, 15 kg of deionized water and 15 g of CF 3 CF 2 CF 2 O(CF(CF 3 )CF 2 O)CF(CF 3 )COONa. Close the reactor, start stirring, evacuate the reactor and replace the atmosphere with nitrogen until the oxygen content of the atmosphere in the reactor is less than 50ppm. At this time, raise the temperature of the reactor to 80°C, and fill the reactor with VDF monomer gas through a membrane pump until the pressure in the reactor is 3.5MPa. 4.6 grams of ethyl acetate and 15 grams of potassium persulfate (made into an aqueous solution) are pumped into the reactor in sequence through a metering pump to initiate polymerization. During the entire polymerization process, gaseous VDF monomer is continuously filled in through a pressure automatic control system to maintain a constant pressure in the reactor at 3.5MPa. Set the VDF monomer gas feed rate to 3.5 kg. When the monomer consumption reaches 25%, add 5 grams of potassium persulfate (made into an aqueous solution) to the reactor. When the monomer consumption reaches 50%, add 5 grams of potassium persulfate (made into an aqueous solution) again. When the specified weight of the mixed gas is added, stop feeding, and the overall reaction time is 2.7 hours. After the reaction is completed, the temperature is lowered to room temperature and the pressure is released. The obtained emulsion is coagulated and washed until the wastewater conductivity is less than 2 μs / cm. The concentrated polymer slurry is spray-dried to obtain a white powder product, which is recorded as PVDF.
[0090] Comparative Example 2
[0091] Preparation of P(VDF-CTFE) copolymer:
[0092] In a 25-liter high-pressure polymerization reactor equipped with a stirrer, 15 kg of deionized water and 15 g of CF 3 CF 2 CF 2 O(CF(CF 3 )CF 2 O)CF(CF 3 )COONa. Close the reactor, start stirring, evacuate the reactor and replace the atmosphere with nitrogen until the oxygen content of the atmosphere in the reactor is less than 50ppm. At this time, the temperature of the reactor is raised to 80°C, and VDF / CTFE mixed monomers are charged into the reactor through a membrane pump until the pressure in the reactor is 3.5MPa. The molar content of VDF in the gaseous monomer mixture is 95 mol%. 4.6 grams of ethyl acetate and 15 grams of potassium persulfate (made into an aqueous solution) are pumped into the reactor in sequence through a metering pump to initiate polymerization. During the entire polymerization process, VDF / CTFE mixed monomers are continuously charged through a pressure automatic control system to maintain a constant pressure in the reactor at 3.5MPa. The VDF / CTFE monomer mixed gas feed rate is set to 3.5 kg. When the monomer consumption reaches 25%, 5 grams of potassium persulfate (made into an aqueous solution) are added to the reactor. When the monomer consumption reaches 50%, 5 grams of potassium persulfate (made into an aqueous solution) are added again. When the specified weight of the mixed gas is added, the feeding is stopped, and the total reaction time is 2.3 hours. After the reaction is completed, the temperature is lowered to room temperature and the pressure is released, and the obtained emulsion is coagulated and washed until the wastewater conductivity is less than 2μs / cm. The concentrated polymer slurry is spray-dried to obtain a white powder product, which is recorded as P(VDF-CTFE).
[0093] The formation of the polymer products prepared in the above Examples 1-3 and Comparative Examples 1-2 was characterized, wherein the weight average molecular weight and molecular weight distribution were characterized by gel permeation chromatography technology; the viscosity was tested using a rotational viscometer, using NMP as a solvent and preparing a solution with a mass concentration of 9.1%; the melting point and crystallization enthalpy were characterized by DSC; and the peel strength was characterized by a 180-degree peeling method using a tensile machine according to the standard method GBT2792-1998.
[0094] The characterization results are summarized in Table 1 below:
[0095] Table 1 Performance test of polymers of Examples 1-3 and Comparative Examples 1-2
[0096]
[0097] The test results show that the grafted vinylidene fluoride copolymer prepared by the method of the present invention can exhibit excellent peel strength, so these materials can effectively improve their bonding strength with electrode active materials and current collectors. The lithium battery prepared with the grafted vinylidene fluoride copolymer as a binder will have outstanding advantages of high peel strength and high cycle capacity retention rate.
Claims
1. A method for preparing a graft-modified fluorinated copolymer, the method comprising: include: Step 1: polymerizing the first monomer and the second monomer to form an intermediate polymer; Step 2: modifying the intermediate polymer using a third monomer to form the grafted fluorinated copolymer; The first monomer is vinylidene fluoride; The second monomer has a structure shown in Formula I: In Formula I, R 1 , R 2 , R 3 and R 4 Each independently selected from: fluorine, chlorine, hydrogen, C1-C6 alkyl optionally substituted by at least one fluorine and / or chlorine, C1-C6 alkoxy optionally substituted by at least one fluorine and / or chlorine, C2-C6 alkenyl optionally substituted by at least one fluorine and / or chlorine, provided that the second monomer contains at least one chlorine atom; The third monomer contains at least one vinyl group and at least one group selected from a carboxylic acid group, a carboxylate group or a carboxylate group.
2. The method according to claim 1, It is characterized in that The molar ratio of the first monomer to the second monomer is 99.9:0.5 to 80:
20.
3. The method according to claim 1, It is characterized in that Based on 100 parts by weight of the total weight of the intermediate polymer, the amount of the third monomer is 0.1 to 20 parts by weight.
4. The method according to claim 1, It is characterized in that The second monomer is selected from one or more of the following: chlorotrifluoroethylene (CTFE), dichlorodifluoroethylene, trichloromonofluoroethylene, chlorodifluoroethylene, chloropentafluoropropylene, dichlorotetrafluoropropylene, trichlorotrifluoropropylene, dichlorotrifluoropropylene, and monochlorotrifluoropropylene.
5. The method according to claim 1, It is characterized in that The third monomer is selected from one or more of the following: acrylic acid, methacrylic acid, itaconic acid, 2-(trifluoromethyl)acrylic acid, acrylate, methacrylate, itaconic acid salt, 2-(trifluoromethyl)acrylate, acrylate (C1-C12) alkyl ester, methacrylate (C1-C12) alkyl ester, itaconic acid (C1-C12) alkyl ester, 2-(trifluoromethyl)acrylate (C1-C12) alkyl ester.
6. The method according to any one of claims 1 to 5, It is characterized in that The method uses one or more additives selected from the group consisting of: emulsifiers, chain transfer agents, initiators.
7. The method according to claim 6, It is characterized in that The emulsifier is selected from one or more of the following: perfluoroalkyl ether carboxylates, perfluoroalkyl carboxylic acids, perfluoropolyether carboxylates, and perfluoroalkyl sulfonamides; The chain transfer agent is selected from one or more of the following: ethyl acetate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethylene carbonate, diethyl malonate, acetone, methyl propionate, ethyl propionate, diethyl succinate; The initiator is selected from one or more of the following: diethylhexyl peroxydicarbonate, tert-butyl peroxyneodecanoate, diisopropyl peroxydicarbonate, dodecyl peroxide, dibenzoyl peroxide, tert-butyl peroxy-2-ethylhexanoate, ammonium persulfate, potassium persulfate, and sodium persulfate.
8. A graft-modified fluorinated copolymer, the fluorinated copolymer being derived from a monomer raw material comprising at least a first monomer, a second monomer and a third monomer, The first monomer is vinylidene fluoride; The second monomer has a structure shown in Formula I: In Formula I, R 1 , R 2 , R 3 and R 4 Each independently selected from: fluorine, chlorine, hydrogen, C1-C6 alkyl optionally substituted by at least one fluorine and / or chlorine, C1-C6 alkoxy optionally substituted by at least one fluorine and / or chlorine, C2-C6 alkenyl optionally substituted by at least one fluorine and / or chlorine, provided that the second monomer contains at least one chlorine atom; The third monomer contains at least one vinyl group and at least one group selected from a carboxylic acid group, a carboxylate group or a carboxylate group; The molar ratio of the first monomer to the second monomer is 99.9:0.5 to 80:20; based on 100 parts by weight of the total weight of the first monomer and the second monomer, the amount of the third monomer is 0.1 to 20 parts by weight; The first monomer and the second monomer are at least partially contained in the main chain of the fluorine-containing copolymer, and the third monomer forms a graft connected to the main chain.
9. The graft-modified fluorinated copolymer according to claim 8, It is characterized in that The graft-modified fluorine-containing copolymer is prepared by the method according to any one of claims 1-7.
10. A binder for a lithium battery, the binder comprising a graft-modified fluorine-containing copolymer prepared by the method of any one of claims 1 to 7, or the binder comprising a graft-modified fluorine-containing copolymer of any one of claims 8 to 9.