Calixarene-based cross-linked polymer as well as synthesis method and application thereof
Through the crosslinked polymer based on cupric aromatic hydrocarbons, the rigid framework formed by its macrocyclic structure and diamine-based crosslinked chain bridge is solved, and the existing lithium ion adsorption materials are insufficiently selected and stable in salt lake brine is achieved. It has efficient lithium ion adsorption and enrichment, and the adsorption capacity reaches 83.68 mg/g.
Patent Information
- Application Number
- CN202411042657.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
AI Technical Summary
Existing lithium ion adsorption materials are insufficient in salt lake brine, making it difficult to efficiently separate and enrich lithium ions, especially in high salinity and repeated adsorption/desorption processes, with poor structural stability.
Using a crosslinked polymer based on cuvities, the crosslinked polymer is formed by repeating structural units cuvities and diamine-based crosslinked chain bridges to form a rigid structural framework, which improves the adsorption capacity and selectivity of lithium ions, and combines specific synthesis methods such as nitro cups. The preparation steps of aromatic hydrocarbons, amino calaric hydrocarbons and crosslinked polymers form materials with high adsorption capacity.
The adsorption capacity and selectivity of lithium ions are significantly improved. The material maintains good structural stability and mechanical properties during high salinity and repeated use, and the adsorption capacity reaches 83.68 mg/g, which is significantly better than the existing technology.
Smart Images

Figure CN118978694A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a cross-linked polymer based on calixarene and a synthesis method and application thereof, belonging to the technical field of polymer materials. Background Art
[0002] Lithium is the metal element with the smallest atomic weight and density. It has good thermal and electrical conductivity and is known as "energy metal", "white oil" and "aerospace alloy". Lithium and its compounds are widely used in metallurgy, energy, medicine, ceramics, electronics and other industries due to their excellent physical and chemical properties.
[0003] With the rapid consumption of fossil energy and the increasingly serious "greenhouse effect", promoting the development of new energy is a key measure to alleviate the energy crisis and achieve the goals of "carbon neutrality and carbon peak". As the focus of the development of the new energy industry, new energy vehicles have developed rapidly in recent years, thus driving a sharp increase in the demand for lithium and its compounds in power batteries.
[0004] In nature, lithium resources are mainly found in granite pegmatite, salt lake brine, underground brine, oilfield brine and seawater. Correspondingly, the lithium extraction technologies developed for various lithium resources include ore lithium extraction technology, brine lithium extraction technology and seawater lithium extraction technology. Due to the low lithium concentration in seawater, only 0.17 mg / L, lithium extraction is difficult and has not been achieved in industrial production so far. Therefore, lithium products mainly come from ore lithium extraction and salt lake lithium extraction, and the lithium output from salt lake lithium extraction accounts for about 60% of the total lithium output.
[0005] Lithium resources in salt lake brine exist in the form of lithium ions in solution. Lithium ions can be selectively extracted directly from the brine, and then lithium carbonate is prepared after evaporation concentration and deep impurity removal. Therefore, compared with the high-energy consumption roasting process required for lithium extraction from ore, lithium extraction from salt lakes has a natural cost advantage.
[0006] Salt lakes can be divided into carbonate salt lakes and non-carbonate salt lakes according to whether the brine contains a large amount of carbonate ions. Carbonate salt lakes have unique components, and the only industrial lithium extraction process suitable for their brine is the "solar pond" method for preparing lithium carbonate concentrate. For non-carbonate salt lake brine, the main processes for extracting lithium from concentrated old brine include precipitation, adsorption, calcination, extraction, electrodialysis, and electrochemical deintercalation.
[0007] The adsorption method is to use Li + The adsorbent material with selective adsorption can absorb Li + Selectively extract and then saturate the adsorbent material with water or acid to remove Li + After desorption, a relatively pure lithium-containing solution is obtained, thus realizing the Li +Effective separation from other impurity ions. The adsorption lithium extraction process is suitable for salt lake brine with high magnesium-lithium ratio and low grade. It has the advantages of simple process, high lithium yield and high selectivity.
[0008] The key to the adsorption method lies in the preparation of the adsorption material. At present, the adsorption materials that can be used for selective lithium extraction from salt lake brine are generally divided into three categories: organic, inorganic and composite adsorption materials. Among them, organic adsorption materials include crown ethers, calixarene, etc., inorganic adsorption materials include aluminum-based adsorbents, lithium ion sieves, natural ores and carbon materials, etc., and composite adsorption materials are organic ligand composite adsorption materials formed by grafting or polymerizing organic ligands onto matrices such as fibers, organic resins, and porous macromolecular materials.
[0009] As a new type of macrocyclic compound with a unique cavity structure, calixarene is called the third generation of supramolecular compounds. The upper edge of calixarene is composed of hydrophobic and lipophilic substituents located in the para position of the hydroxyl group of the benzene ring, the lower edge is composed of a tight and regular combination of hydrophilic phenolic hydroxyl groups, and the middle is composed of a hydrophobic cavity with electrons formed by the benzene ring. Calixarene has the following characteristics: ① Different cavities of different sizes can be obtained according to needs; ② Different conformations can be obtained under different reaction conditions; ③ Various derivatives can be obtained through organic synthesis. Therefore, as a highly selective host molecule, calixarene can form complexes with neutral molecules, organic molecules, etc. In addition, since calixarene itself has multiple hydroxyl groups and an electron hole, calixarene and its derivatives can form complexes with almost all metal cations, which makes this substance achieve rapid development in the research of metal ion complexation.
[0010] Previous studies have shown that various types of calixarene derivatives have a + The selectivity and adsorption of Li2O3 indicated that esters had the best competitiveness, ethers had the highest extraction rate, and amide esters had the best selectivity. + The selectivity is the strongest and the thermal stability is relatively high, which is beneficial to Li + Therefore, ion imprinting technology or molecular sieves can be used to polymerize ester-based calixarene derivative monomers with good selectivity to synthesize Li + The invention discloses a brine lithium extraction adsorption material which has strong regeneration, long service life, good specific adsorption effect, large adsorption capacity, uniform particle size and can realize continuous operation in the separation and extraction process.
[0011] It has been reported that tert-butyl calix[4]arene oxoacetic acid was used as the functional monomer, lithium ions were used as the template ions, and n-butyl titanate was used as the crosslinking agent. The ion imprinting technology was used to prepare calixarene lithium ion imprinted polymer. The optimal adsorption conditions were: temperature 28°C, pH 8, acid washing concentration 1 mol / L, dosage 40 ml, and the saturated adsorption capacity reached 22.53 mg / g when the optimal adsorption time was 6 h. Interfering ions Mg 2+ , Ca 2+ 、Na + , K + The selectivity and adsorption capacity of the calixarene lithium ion imprinted polymer have basically no effect. The reusability of the calixarene lithium ion imprinted polymer is high. After five uses, its adsorption effect only decreases by 5%, the adsorption activity remains at 97.2% of the original, and the mass loss is about 17%. It can be concluded that the polymer has good regeneration and reusability.
[0012] There are also reports that cellulose nanocrystals are used as templates, doped with imprinted carboxy azo calix [4] arene, and a silicon dioxide film is synthesized by a simple evaporation self-assembly method. Then, the imprinted calix [4] arene is loaded on the surface of the silicon film by an impregnation method to obtain a double imprinted porous silicon film. The adsorption capacity of this material for lithium ions can reach 16.07 mg / g at pH = 6.0 and temperature of 25°C. After 5 adsorption-desorption cycles, the adsorption capacity is about 85% of the first time, showing excellent regeneration efficiency. There are also carbon nanotubes, γ-glycidyloxypropyltrimethoxysilane, and tert-butyl calix [4] arene as raw materials, combined with ion imprinting technology, and a kind of imprinted porous adsorption material is obtained by chemical bonding. The adsorption performance of lithium ions is roughly the same as that of the above double imprinted silicon film.
[0013] Chinese patent CN115403721 B discloses a method for preparing a covalent organic framework material for lithium isotope separation and its application. The invention introduces the concept of covalent organic framework materials and calixarene functional groups into the work of lithium isotope separation. Since this type of material can provide a higher density of adsorption sites for lithium ions by constructing periodic structural units, and calixarene can provide a higher lithium ion binding ability and lithium isotope separation effect, compared with other types of solid-phase adsorption materials, the adsorption performance of lithium ions and the separation performance of lithium isotopes can be significantly improved. The prepared material has a high level of lithium ion adsorption capacity (saturated adsorption capacity 94.66 mg / g) and lithium isotope separation ability (separation coefficient 1.053). When preparing the above covalent organic framework material, first take calixarene and hexamethylenetetramine, add them to trifluoroacetic acid solvent at the same time, fully react at 80°C to 90°C for 18h to 24h, cool to room temperature after the reaction, extract, and distill under reduced pressure to obtain a aldehyde-formyl calixarene monomer; then take the obtained aldehyde-formyl calixarene monomer and mix it with a benzidine monomer, pre-treat it with ultrasound for 5min to 10min, then add acetic acid aqueous solution as a catalyst, ultrasonically pre-treat it at an ultrasonic frequency of 60-80KHz for 3min to 5min, then add a solvent, fully react at 110°C to 130°C for 60h to 72h, filter and collect the precipitated product after the reaction, use anhydrous methanol or ethanol to extract it with Soxhlet, and vacuum dry it to obtain a covalent organic framework material for lithium isotope separation.
[0014] Chinese patent CN103055816 A discloses a novel type of calixarene crown ether bonded silicon-based adsorbent material and its preparation method. The adsorbent material has a structure shown in the following formula:
[0015]
[0016] Wherein, X = 2-12, R = H or
[0017] When preparing the above-mentioned adsorbent material, firstly, di(2-propoxy)calix[4]arene-crown 6 is modified so that its molecular structure has a reactive amine group, and then a silicon-based precursor containing a haloalkyl group is prepared: finally, the amino-substituted di(2-propoxy)calix[4]arene-crown 6 is reacted with the haloalkyl-containing silicon-based precursor, thereby bonding the calixarene crown ether group to the silicon-based carrier to obtain a new type of calixarene crown ether bonded silicon-based adsorbent material.
[0018] In summary, with the development of lithium extraction technology from salt lakes, adsorption materials, as the core of adsorption methods, are ushering in a new era. Ideal adsorption materials should have the following characteristics: 1) High selectivity, which can selectively capture Li from solutions with complex element composition and high salinity. +; 2) Good stability, maintaining good structural stability and mechanical stability under high salinity and repeated adsorption / desorption processes; 3) Sufficient adsorption capacity, that is, the unit mass of adsorption material can capture as many lithium ions as possible. Summary of the invention
[0019] In view of the shortcomings of the prior art, the object of the present invention is to provide a lithium ion adsorption material with high selectivity, good stability and sufficient adsorption capacity.
[0020] Another object of the present invention is to provide a method for synthesizing the lithium ion adsorption material.
[0021] Another object of the present invention is to provide the lithium ion adsorption material for use in a salt lake lithium extraction system to separate and enrich lithium metal ions.
[0022] To achieve the above object, the present invention provides a cross-linked polymer based on calixarene, which is composed of the following repeating structural units of calixarene and diamine cross-linked bridges, and has a number average molecular weight of 7500 to 15000.
[0023]
[0024] Wherein, n is the number of repetitions of the methylene phenol unit in the calixarene, and the cross-linking bridge is a diamine group -NH-R-NH-, one end of which is connected to the para position of the methylene phenol unit of the calixarene, and the other end is connected to the para position of another methylene phenol unit of the calixarene, and this is repeated.
[0025] The R group in the cross-linked chain bridge diamine group -NH-R-NH- includes a propane group, a diethyl ether group, a phenyl group, or a triazine group, preferably an aromatic phenyl group. This rigid structural skeleton makes the lithium ions less susceptible to the influence of solvents or thermal motion at the adsorption sites, thereby greatly improving the adsorption capacity of lithium ions.
[0026] The number of repetitions of the methylene phenol unit in the calixarene includes n=1, 3 or 5, that is, the repeating structural unit calixarene is calix[4]arene, calix[6]arene or calix[8]arene, preferably, the number of repetitions of the methylene phenol unit in the calixarene is n=1, that is, the repeating structural unit calixarene is calix[4]arene. The adsorption capacity of calixarene for metal ions is mainly determined by the macrocyclic structure of calixarene. The hydroxyl group of calix[4]arene forms a ring with a diameter of The adsorption holes can induce the specific adsorption of lithium ions.
[0027] The above-mentioned synthesis method based on calixarene cross-linked polymer comprises the following steps:
[0028] A) preparing nitrocalixarene, comprising:
[0029] (A1) weighing tert-butylcalixarene monomer and anhydrous organic solvent to prepare a mixed solution with a molar ratio of 1:3 to 5;
[0030] (A2) adding 1 to 3 times the amount of glacial acetic acid and 4 to 10 times the amount of fuming nitric acid in the amount of tert-butylcalixarene monomer, mixing well, and reacting at 0°C to 50°C for 2h to 8h;
[0031] After the reaction (A3) is completed, the mixture is allowed to stand for clarification, and the phases are separated. The upper organic phase is evaporated in vacuo to obtain a solid precipitate, which is washed with an anhydrous organic solvent corresponding to A1 until the washing liquid is neutral to obtain nitrocalixarene, whose chemical structure is:
[0032]
[0033] B) preparing aminocalixarene, comprising:
[0034] (B1) weighing the nitrocalixarene prepared in step A and an anhydrous organic solvent to prepare a mixed solution with a molar ratio of 1:3 to 6;
[0035] (B2) adding a palladium-carbon catalyst to the reaction system under a saturated nitrogen atmosphere with a water-oxygen concentration of less than 10 ppm;
[0036] (B3) firstly introducing hydrogen to replace the original nitrogen atmosphere, and then using a circulating ventilation device to continuously introduce hydrogen to carry out a hydrogenation reduction reaction, maintaining a temperature of 20° C. to 50° C. for a reaction of 20.0 h to 48.0 h;
[0037] (B4) After the reaction is completed, water is first injected to terminate the catalytic reaction of the palladium-carbon catalyst, and then the upper organic phase is taken and allowed to stand for phase separation and evaporated in vacuum to obtain aminocalixarene, whose chemical structure is:
[0038]
[0039] C) preparing a crosslinked polymer based on calixarene, comprising:
[0040] (C1) weighing the aminocalixarene described in step B and mixing it with an anhydrous solvent to prepare a mixed solution with a molar ratio of 1:3 to 6;
[0041] (C2) adding a cross-linking agent in an amount of 1 / 8 to 1 / 6 of the aminocalixarene substance and mixing well;
[0042] (C3) adding a condensation aid in an amount of 1 / 10 to 1 / 7 of the amount of the aminocalix aromatic substance to carry out a condensation polymerization reaction, maintaining a temperature of 60° C. to 100° C. for 48.0 h to 96 h;
[0043] (C4) After the reaction is completed, the solid product is obtained by liquid-solid separation, and the solid product is washed more than 3 times with the corresponding anhydrous solvent in step C1, and the solid product is separated from the liquid and dried at 60° C. to obtain the above-mentioned calixarene-based cross-linked polymer.
[0044] Generally, anhydrous organic solvents include benzene, toluene, dichloromethane and chloroform, which can be prepared by dehydration methods such as redistillation or molecular sieves.
[0045] In step A, the tert-butylcalixarene monomer includes tert-butylcalix[4]arene, tert-butylcalix[6]arene and tert-butylcalix[8]arene, and the general chemical structure thereof is:
[0046]
[0047] Here, n is the number of repetitions of the methylenephenol unit in the calixarene.
[0048] In step B, the palladium carbon catalyst uses a palladium carbon catalyst with an effective substance mass percentage of 5% and water added to a mass percentage of 50%.
[0049] In step C, the cross-linking agent includes 1,3-dichloropropane, 2,2-dichloroethyl ether, 1,4-dichlorobenzene and 2,4-dichloro-1,3,5-triazine, and the condensation auxiliary agent includes sodium bicarbonate, sodium carbonate, sodium hydroxide and triethylamine.
[0050] The calixarene-based cross-linked polymer can be used to separate and enrich lithium ions in salt lake brine.
[0051] Compared with the prior art, the present invention has the following beneficial effects:
[0052] 1. The adsorption capacity of the cross-linked polymer based on calixarene of the present invention for lithium ions reaches 83.68 mg / g, which has significant advantages over the lithium ion adsorption materials in the prior art. The cross-linked bridge in the cross-linked polymer based on calixarene of the present invention is a diamine group -NH-R-NH-, wherein the R group is a propane group, a diethyl ether group, a phenyl group, a triazine group, etc., which are all small molecular groups with a small molecular weight and a low proportion of bridges, thereby highlighting that the cross-linked polymer of calixarene has a higher proportion of calixarene functional groups with adsorption capacity and more adsorption sites, thereby improving the adsorption capacity for lithium ions; on the other hand, the cross-linked polymer based on calixarene uses aromatic phenylenediamine groups to achieve cross-linking. This rigid structural skeleton makes lithium ions less susceptible to solvent or thermal motion at the adsorption sites, thereby greatly improving the adsorption capacity for lithium ions.
[0053] 2. The cross-linked polymer based on calixarene of the present invention has high selectivity for lithium ion adsorption. The adsorption capacity of calixarene for metal ions is mainly determined by the macrocyclic structure of calixarene. The hydroxyl group of calix[4]arene forms a nanostructure with a diameter of adsorption holes, inducing specific adsorption of lithium ions.
[0054] 3. The cross-linked polymer based on calixarene of the present invention is obtained by chemically modifying tert-butylcalixarene to form a calixarene with an active center, and then undergoing an acid-ammonia condensation reaction to obtain a cross-linked polymer. The cross-linked polymer is a polymer with a three-dimensional network structure, is insoluble, and does not melt. Its mechanical properties, thermal stability, solvent resistance, and creep resistance are greatly improved, and it has good stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0055] Figure 1 It is the general chemical structure formula of a cross-linked polymer based on calixarene.
[0056] Figure 2 NMR of polycalix[4]arene 2,4-dichloro-1,3,5-triazine and 2,4,6-trichloro-1,3,5-triazine 13 C spectrum.
[0057] Figure 3 This is the SEM image of polycalix[4]arene 2,4-dichloro-1,3,5-triazine.
[0058] Figure 4 This is the SEM image of polycalix[4]arene 2,4,6-trichloro-1,3,5-triazine. DETAILED DESCRIPTION
[0059] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that these descriptions are exemplary only and are not intended to limit the scope of the present invention. In addition, in the following description, the description of known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.
[0060] The present invention provides a cross-linked polymer based on calixarene, the chemical structure of which is as follows: Figure 1 It is shown that it is composed of repeating structural units of calixarene and diamine cross-linked bridges, wherein n is the number of repetitions of the methylene phenol unit in the calixarene, and the cross-linked bridge is a diamine group -NH-R-NH-, one end of which is connected to the para position of the calixarene methylene phenol unit, and the other end is connected to the para position of another calixarene methylene phenol unit, and so on.
[0061] The R group in the cross-linked chain bridge diamine group -NH-R-NH- includes a propane group, a diethyl ether group, a phenyl group, or a triazine group, preferably an aromatic phenyl group. This rigid structural skeleton makes the lithium ions less susceptible to the influence of solvents or thermal motion at the adsorption sites, thereby greatly improving the adsorption capacity of lithium ions.
[0062] The number of repetitions of the methylene phenol unit in the calixarene includes n=1, 3 or 5, that is, the repeating structural unit calixarene is calix[4]arene, calix[6]arene or calix[8]arene, preferably, the number of repetitions of the methylene phenol unit in the calixarene is n=1, that is, the repeating structural unit calixarene is calix[4]arene. The adsorption capacity of calixarene for metal ions is mainly determined by the macrocyclic structure of calixarene. The hydroxyl group of calix[4]arene forms a ring with a diameter of The adsorption holes can induce the specific adsorption of lithium ions.
[0063] Figure 2 NMR of polycalix[4]arene 2,4-dichloro-1,3,5-triazine and 2,4,6-trichloro-1,3,5-triazine 13 C spectrum.
[0064] Figure 3 This is the SEM image of polycalix[4]arene 2,4-dichloro-1,3,5-triazine.
[0065] Figure 4 This is the SEM image of polycalix[4]arene 2,4,6-trichloro-1,3,5-triazine.
[0066] The above-mentioned synthesis method based on calixarene cross-linked polymer comprises the following steps:
[0067] A) preparing nitrocalixarene, comprising:
[0068] (A1) weighing tert-butylcalixarene monomer and anhydrous organic solvent to prepare a mixed solution with a molar ratio of 1:3 to 5;
[0069] (A2) adding 1 to 3 times the amount of glacial acetic acid and 4 to 10 times the amount of fuming nitric acid in the amount of tert-butylcalixarene monomer, mixing well, and reacting at 0°C to 50°C for 2h to 8h;
[0070] After the reaction (A3) is completed, the mixture is allowed to stand for clarification, and the phases are separated. The upper organic phase is evaporated in vacuo to obtain a solid precipitate, which is washed with an anhydrous organic solvent corresponding to A1 until the washing liquid is neutral to obtain nitrocalixarene, whose chemical structure is:
[0071]
[0072] B) preparing aminocalixarene, comprising:
[0073] (B1) weighing the nitrocalixarene prepared in step A and an anhydrous organic solvent to prepare a mixed solution with a molar ratio of 1:3 to 6;
[0074] (B2) adding a palladium-carbon catalyst to the reaction system under a saturated nitrogen atmosphere with a water-oxygen concentration of less than 10 ppm;
[0075] (B3) firstly introducing hydrogen to replace the original nitrogen atmosphere, and then using a circulating ventilation device to continuously introduce hydrogen to carry out a hydrogenation reduction reaction, maintaining a temperature of 20° C. to 50° C. for a reaction of 20.0 h to 48.0 h;
[0076] (B4) After the reaction is completed, water is first injected to terminate the catalytic reaction of the palladium-carbon catalyst, and then the upper organic phase is taken and allowed to stand for phase separation and evaporated in vacuum to obtain aminocalixarene, whose chemical structure is:
[0077]
[0078] C) preparing a crosslinked polymer based on calixarene, comprising:
[0079] (C1) weighing the aminocalixarene described in step B and mixing it with an anhydrous solvent to prepare a mixed solution with a molar ratio of 1:3 to 6;
[0080] (C2) adding a cross-linking agent in an amount of 1 / 8 to 1 / 6 of the aminocalixarene substance and mixing well;
[0081] (C3) adding a condensation aid in an amount of 1 / 10 to 1 / 7 of the amount of the aminocalix aromatic substance to carry out a condensation polymerization reaction, maintaining a temperature of 60° C. to 100° C. for 48.0 h to 96 h;
[0082] (C4) After the reaction is completed, the solid product is obtained by liquid-solid separation, and the solid product is washed more than 3 times with the corresponding anhydrous solvent in step C1, and the solid product is separated from the liquid and dried at 60° C. to obtain the above-mentioned calixarene-based cross-linked polymer.
[0083] Generally, anhydrous organic solvents include benzene, toluene, dichloromethane and chloroform, which can be prepared by dehydration methods such as redistillation or molecular sieves.
[0084] In step A, the tert-butylcalixarene monomer includes tert-butylcalix[4]arene, tert-butylcalix[6]arene and tert-butylcalix[8]arene, and the general chemical structure thereof is:
[0085]
[0086] Here, n is the number of repetitions of the methylenephenol unit in the calixarene.
[0087] In step B, the palladium carbon catalyst uses a palladium carbon catalyst with an effective substance mass percentage of 5% and water added to a mass percentage of 50%.
[0088] In step C, the cross-linking agent includes 1,3-dichloropropane, 2,2-dichloroethyl ether, 1,4-dichlorobenzene and 2,4-dichloro-1,3,5-triazine, and the condensation auxiliary agent includes sodium bicarbonate, sodium carbonate, sodium hydroxide and triethylamine.
[0089] Some synthesis examples of the calixarene-based crosslinked polymer are further listed below.
[0090]
Example 1
[0091] First, 0.1 mol of tert-butylcalix[6]arene monomer and anhydrous solvent dichloromethane are weighed to prepare a mixed solution with a molar ratio of 1:3, 1 times the amount of glacial acetic acid and 6 times the amount of fuming nitric acid of the tert-butylcalix[6]arene monomer are added, mixed evenly, maintained at 0°C for sufficient reaction for 8 hours, and after the reaction is completed, allowed to stand for clarification, phase separation, and the upper organic phase is vacuum evaporated to obtain a solid precipitate, which is washed with the corresponding anhydrous solvent dichloromethane until the washing liquid is neutral to obtain nitrocalix[6]arene.
[0092] Then, 0.1 mol of the above-mentioned nitrocalix[6]arene was weighed and mixed with anhydrous solvent dichloromethane to prepare a mixed solution with a molar ratio of 1:4. 1 g of 5% wet palladium carbon (50% water) was added to the reaction system under a saturated nitrogen atmosphere (water and oxygen concentration was less than 10 ppm). First, hydrogen was introduced to replace the original nitrogen atmosphere, and then hydrogen was continuously introduced using a circulating aeration device to carry out a hydrogenation amination reduction reaction. The reaction was maintained at 30° C. for 24.0 hours. After the reaction was completed, water was first injected to terminate the catalysis of the palladium carbon catalyst, and then the upper organic phase of the static phase separation was evaporated in vacuo to obtain aminocalix[6]arene.
[0093] Finally, 0.1 mol of the aminocalix[6]arene was weighed and mixed with anhydrous solvent toluene to prepare a mixed solution with a molar ratio of 1:4, and a crosslinking agent 2,4-dichloro-1,3,5-triazine was added, and the molar ratio of aminocalix[6]arene to 2,4-dichloro-1,3,5-triazine was 1:8. The mixture was evenly mixed, and then a condensation auxiliary agent triethylamine was added, and the molar ratio of aminocalix[6]arene to triethylamine was 1:8. The condensation reaction was carried out, and the temperature was maintained at 100° C. for full reaction for 48.0 hours. After the reaction was completed, a solid product was obtained by liquid-solid separation, and the solid product was repeatedly washed with anhydrous solvent toluene, and the liquid-solid separation was carried out. The crosslinked polymer based on calix[6]arene, namely polycalix[6]arene-2,4-dichloro-1,3,5-triazine, was obtained by vacuum drying at 60° C. The number average molecular weight (Mn) of the obtained polycalix[6]arene-2,4-dichloro-1,3,5-triazine was 15,000 by gel permeation chromatography (GPC).
[0094]
Example 2
[0095] First, 0.1 mol of tert-butylcalix[6]arene monomer is weighed and mixed with anhydrous solvent toluene to prepare a mixed solution with a molar ratio of 1:5, 1 times the amount of glacial acetic acid and 4 times the amount of fuming nitric acid of the tert-butylcalix[6]arene monomer are added, mixed evenly, maintained at 40° C. for full reaction for 10 hours, and after the reaction is completed, allowed to stand for clarification, phase separation, and the upper organic phase is vacuum evaporated to obtain a solid precipitate, which is washed with the corresponding anhydrous solvent toluene until the washing liquid is neutral to obtain nitrocalix[6]arene.
[0096] Then, 0.1 mol of the above-mentioned nitrocalix[6]arene was weighed and mixed with anhydrous solvent toluene to prepare a mixed solution with a molar ratio of 1:6, and 1 g of 5% wet palladium carbon (50% water) was added to the reaction system under a saturated nitrogen atmosphere (water and oxygen concentration was less than 10 ppm). First, hydrogen was introduced to replace the original nitrogen atmosphere, and then hydrogen was continuously bubbled into the system using a circulating aeration device for hydrogenation amination reduction reaction. The temperature was maintained at 20°C for 20.0 hours to fully react. After the reaction was completed, water was first injected to terminate the catalysis of the palladium carbon catalyst, and then the upper organic phase of the static phase separation was evaporated in vacuo to obtain aminocalix[6]arene.
[0097] Finally, 0.1 mol of the aminocalix[6]arene was weighed and mixed with anhydrous solvent toluene to prepare a mixed solution with a molar ratio of 1:3, and a crosslinking agent 1,3-dichloropropane was added, and the molar ratio of aminocalix[6]arene to 1,3-dichloropropane was 1:6. The mixture was mixed evenly, and then a condensation auxiliary agent sodium carbonate was added, and the molar ratio of aminocalix[6]arene to sodium carbonate was 1:8. The condensation reaction was carried out, and the temperature was maintained at 80°C for full reaction for 72.0 hours. After the reaction was completed, the solid product was separated by liquid-solid separation, and the solid product was repeatedly washed with anhydrous solvent toluene, and the solid-liquid separation was carried out. The crosslinked polymer based on calix[6]arene-1,3-dichloropropane was obtained by freeze-drying at 60°C. The number average molecular weight (Mn) of the obtained polycalix[6]arene-1,3-dichloropropane was 7500 after analysis by gel permeation chromatography (GPC).
[0098]
Example 3
[0099] First, 0.1 mol of tert-butylcalix[4]arene monomer and anhydrous solvent chloroform are weighed to prepare a mixed solution with a molar ratio of 1:3, 2 times the amount of glacial acetic acid and 8 times the amount of fuming nitric acid of the tert-butylcalix[4]arene monomer are added, mixed evenly, maintained at 20° C. for sufficient reaction for 4 hours, and after the reaction is completed, allowed to stand for clarification, phase separation, and the upper organic phase is vacuum evaporated to obtain a solid precipitate, which is washed with the corresponding anhydrous solvent chloroform until the washing liquid is neutral to obtain nitrocalix[4]arene.
[0100] Then, 0.1 mol of the above-mentioned nitrocalix[4]arene was weighed and mixed with anhydrous solvent chloroform to prepare a mixed solution with a molar ratio of 1:3. 1 g of 5% wet palladium carbon (50% water) was added to the reaction system under a saturated nitrogen atmosphere (water and oxygen concentration was less than 10 ppm). First, hydrogen was introduced to replace the original nitrogen atmosphere, and then hydrogen was continuously introduced using a circulating aeration device to carry out a hydrogenation amination reduction reaction. The temperature was maintained at 20°C for 48.0 hours to fully react. After the reaction was completed, water was first injected to terminate the catalysis of the palladium carbon catalyst, and then the upper organic phase of the static phase separation was evaporated in vacuum to obtain aminocalix[4]arene.
[0101] Finally, 0.1 mol of aminocalix[4]arene was weighed and mixed with anhydrous solvent benzene to prepare a mixed solution with a molar ratio of 1:6, and a crosslinking agent 1,4-dichlorobenzene was added, and the molar ratio of aminocalix[4]arene to 1,4-dichlorobenzene was 1:6. The mixture was mixed evenly, and then a condensation auxiliary agent sodium bicarbonate was added, and the molar ratio of aminocalix[4]arene to sodium bicarbonate was 1:7. The condensation reaction was carried out, and the temperature was maintained at 62°C for full reaction for 96.0 hours. After the reaction was completed, the solid product was separated by liquid-solid separation, and the solid product was repeatedly washed with anhydrous solvent benzene, and the solid product was separated by liquid-solid separation. The crosslinked polymer based on calixarene, polycalix[4]arene-1,4-dichlorobenzene, was obtained by freeze-drying at 60°C. The number average molecular weight (Mn) of the obtained polycalix[4]arene-1,4-dichlorobenzene was 13000 after analysis by gel permeation chromatography (GPC).
[0102]
Example 4
[0103] First, 0.1 mol of tert-butylcalix[4]arene monomer and anhydrous solvent dichloromethane are weighed to prepare a mixed solution with a molar ratio of 1:4, 1 times the amount of glacial acetic acid and 10 times the amount of fuming nitric acid of the tert-butylcalix[4]arene monomer are added, mixed evenly, maintained at 40° C. for sufficient reaction for 2 hours, and after the reaction is completed, allowed to stand for clarification, phase separation, and the upper organic phase is vacuum evaporated to obtain a solid precipitate, which is washed with the corresponding anhydrous solvent dichloromethane until the washing liquid is neutral to obtain nitrocalix[4]arene.
[0104] Then, 0.1 mol of the above-mentioned nitrocalix[4]arene was weighed and mixed with anhydrous solvent dichloromethane to prepare a mixed solution with a molar ratio of 1:5. 1 g of 5% wet palladium carbon (50% water) was added to the reaction system under a saturated nitrogen atmosphere (water and oxygen concentration was less than 10 ppm). First, hydrogen was introduced to replace the original nitrogen atmosphere, and then hydrogen was continuously introduced using a circulating aeration device to carry out a hydrogenation amination reduction reaction. The reaction was maintained at 30°C for 30.0 hours. After the reaction was completed, water was first injected to terminate the catalysis of the palladium carbon catalyst, and then the upper organic phase of the static phase separation was evaporated in vacuo to obtain aminocalix[4]arene.
[0105] Finally, 0.1 mol of the aminocalix[4]arene was weighed and mixed with anhydrous solvent toluene to prepare a mixed solution with a molar ratio of 1:5, and a crosslinking agent 2,2-dichloroethyl ether was added, and the molar ratio of aminocalix[4]arene to 2,2-dichloroethyl ether was 1:8, and the mixture was mixed evenly, and then a condensation auxiliary agent sodium bicarbonate was added, and the molar ratio of aminocalix[4]arene to sodium bicarbonate was 1:10, and a condensation reaction was carried out, and the reaction was fully carried out at 80° C. for 60.0 hours. After the reaction was completed, a solid product was obtained by liquid-solid separation, and the solid product was repeatedly washed with anhydrous solvent toluene, and the solid-liquid separation was carried out, and the solid product was freeze-dried at 62° C. to obtain a crosslinked polymer based on calixarene, namely polycalix[4]arene-2,2-dichloroethyl ether. The crosslinked polymer was analyzed by gel permeation chromatography (GPC), and the number average molecular weight (Mn) of the obtained polycalix[4]arene-2,2-dichloroethyl ether was 8300.
[0106]
Example 5
[0107] First, 0.1 mol of tert-butylcalix[8]arene monomer and anhydrous solvent chloroform are weighed to prepare a mixed solution with a molar ratio of 1:3, 3 times the amount of glacial acetic acid and 5 times the amount of fuming nitric acid of the tert-butylcalix[8]arene monomer are added, mixed evenly, maintained at 50° C. for sufficient reaction for 2 hours, and after the reaction is completed, allowed to stand for clarification, phase separation, and the upper organic phase is vacuum evaporated to obtain a solid precipitate, which is washed with the corresponding anhydrous solvent chloroform until the washing liquid is neutral to obtain nitrocalix[8]arene.
[0108] Then, 0.1 mol of the above-mentioned nitrocalix[8]arene was weighed and mixed with anhydrous solvent chloroform to prepare a mixed solution with a molar ratio of 1:6. 1 g of 5% wet palladium carbon (50% water) was added to the reaction system under a saturated nitrogen atmosphere (water and oxygen concentration was less than 10 ppm). First, hydrogen was introduced to replace the original nitrogen atmosphere, and then hydrogen was continuously introduced using a circulating aerator to carry out a hydrogenation amination reduction reaction. The reaction was maintained at 50° C. for 35.0 hours. After the reaction was completed, water was first injected to terminate the catalysis of the palladium carbon catalyst, and then the upper organic phase of the static phase separation was evaporated in vacuo to obtain aminocalix[8]arene.
[0109] Finally, 0.1 mol of the aminocalix[8]arene was weighed and mixed with anhydrous solvent chloroform to prepare a mixed solution with a molar ratio of 1:4, and a crosslinking agent 2,4-dichloro-1,3,5-triazine was added, and the molar ratio of aminocalix[8]arene to 2,4-dichloro-1,3,5-triazine was 1:6. The mixture was mixed evenly, and then a condensation auxiliary agent sodium hydroxide was added, and the molar ratio of aminocalix[8]arene to sodium hydroxide was 1:8. The condensation reaction was carried out, and the temperature was maintained at 62° C. for full reaction for 96.0 hours. After the reaction was completed, a solid product was obtained by liquid-solid separation, and the solid product was repeatedly washed with anhydrous solvent chloroform, and the liquid-solid separation was carried out. The crosslinked polymer based on calixarene, polycalix[8]arene-2,4-dichloro-1,3,5-triazine, was obtained by hot air drying at 60° C. The number average molecular weight (Mn) of the obtained polycalix[8]arene-2,4-dichloro-1,3,5-triazine was 11,000 by gel permeation chromatography (GPC).
[0110] [Comparative Example]
[0111] Conventional unmodified aluminum-based adsorbents were prepared using a co-precipitation method.
[0112] 0.5 mol LiCl salt, 1 mol AlCl 3 The salt was prepared in 100 ml of aqueous solution, and 20 ml of 8 mol / L NaOH solution was prepared. The lithium aluminum aqueous solution was added dropwise into the hot NaOH solution with high-speed stirring at a speed of 350 rpm and a temperature of 80 degrees Celsius. After multiple water washing, vacuum distillation, and freeze drying, [LiAl 2 (OH) 6 ]X n- 1-n ·mH 2 O Aluminum-based adsorbent.
[0113] [Simulation test of lithium extraction from salt lake]
[0114] Simulated salt lake brine: Na + 99.32g / L, Mg 2+ 16.8g / L, Li + 0.79g / L, Cl - 198.4g / L, K + 16.7g / L, SO 4 2- 21.1g / L, pH 7.32.
[0115] Test method:
[0116] The adsorbent materials were placed in a group of simulated salt lake brine (pre-adsorption solution) and stirred for adsorption at a temperature of 15°C, a stirring speed of 300 r / min, and an adsorption time of 2 h. After the adsorption was completed, vacuum filtration was performed to obtain the post-adsorption solution and the loaded adsorbent material.
[0117] Take the above-mentioned loaded adsorbent material, desorb it with a hydrochloric acid solution with a concentration of 1 mol / L at a rotation speed of 300 r / min and a desorption time of 2 h. After the desorption is completed, vacuum filtration is performed to obtain a desorption solution and an unloaded adsorbent material.
[0118] The element concentrations in the solution before adsorption, the solution after adsorption and the desorption solution were determined by ICP-MS.
[0119] The adsorption capacity of the adsorbent material for lithium ions is calculated according to the following formula:
[0120] Q t =(C 0 -C t )×V / m
[0121] Among them, Q t ——Adsorption capacity, C 0 ——Lithium ion concentration of solution before adsorption, C t ——Lithium ion concentration of the solution after adsorption, V——volume of the solution, m——mass of the adsorption material.
[0122] The cross-linked polymers based on calixarene obtained in Examples 1 to 5 and the conventional unmodified aluminum-based adsorbent prepared by the coprecipitation method in the comparative example were used to carry out a simulation test on lithium extraction from salt lakes. The test results are shown in Tables 1 and 2.
[0123] Table 1 Adsorption capacity of adsorbent materials for lithium ions, mg / g
[0124]
[0125] Table 2 Element concentrations in analytical solutions, g / L
[0126]
[0127] Test conclusion:
[0128] 1) The adsorption capacity of lithium ions in brine by the cross-linked polymer based on calixarene of the present invention can reach 83.68 mg / g, which has significant advantages over existing lithium ion adsorption materials such as inorganic aluminum-based adsorbents with LDH structure (with a lithium ion adsorption capacity of 4.0 mg / g to 8 mg / g). The cross-linked bridge in the cross-linked polymer based on calixarene is a diamine group -NH-R-NH-, in which the R group is a propane group, a diethyl ether group, a phenyl group, a triazine group, etc., which are all small molecular groups with small molecular weights and low bridge ratios, thereby highlighting that the cross-linked polymer of calixarene has a higher proportion of calixarene functional groups with adsorption capacity and more adsorption sites, thereby improving the adsorption capacity for lithium ions.
[0129] 2) Compared with the carbon chain structure, the aromatic phenyl structure can make the cross-linked polymer based on calixarene have better lithium ion adsorption performance. This can be attributed to the rigid structural skeleton of the phenyl group, which makes the lithium ions less susceptible to the influence of solvent or thermal motion at the adsorption site, thereby improving the adsorption capacity of lithium ions. As shown in Table 1, Example 1 and Example 2, Example 3 and Example 4, the former has an aromatic phenyl structure, and the latter is an aliphatic pre-loaded structure. The adsorption capacity of the former is higher than that of the latter, and the effect is very significant.
[0130] 3) The metal ion adsorption capacity of calixarene polymers is mainly determined by the calixarene macrocyclic structure. The hydroxyl groups of calix[4]arene can form a The adsorption holes induce the specific adsorption of lithium ions. As shown in Table 2, calix[6]arene has a higher adsorption rate for sodium ions, calix[8]arene has a higher adsorption rate for potassium ions, and dicalix[4]arene has a higher adsorption rate for magnesium ions.
[0131] In summary, the cross-linked polymer based on calixarene in the present invention is applied to separate and enrich lithium ions in a salt lake lithium extraction system, and has broad application prospects.
[0132] It should be understood that the above specific embodiments of the present invention are only used to illustrate or explain the principles of the present invention, and do not constitute a limitation of the present invention. Therefore, any modifications, equivalent substitutions, improvements, etc. made without departing from the spirit and scope of the present invention should be included in the protection scope of the present invention. In addition, the appended claims of the present invention are intended to cover all changes and modifications that fall within the scope and boundaries of the appended claims, or the equivalent forms of such scope and boundaries.
Claims
1. A cross-linked polymer based on calixarene, characterized in that: The cross-linked polymer based on calixarene is composed of the following repeating structural units: calixarene and diamine cross-linked bridges, and has a number average molecular weight of 7500 to 15000. Wherein, n is the number of repetitions of the methylene phenol unit in the calixarene, and the cross-linking bridge is a diamine group -NH-R-NH-, one end of which is connected to the para position of the methylene phenol unit of the calixarene, and the other end is connected to the para position of another methylene phenol unit of the calixarene, and this is repeated.
2. The cross-linked polymer based on calixarene according to claim 1, characterized in that The R group in the cross-linked chain bridge diamine group -NH-R-NH- includes a propane group, a diethyl ether group, a phenyl group, and an s-triazine group, and is preferably an aromatic phenyl group.
3. The cross-linked polymer based on calixarene according to claim 2, characterized in that The repetition number of the methylene phenol unit in the calixarene includes n=1, 3 or 5, that is, the repeating structural unit calixarene is calix[4]arene, calix[6]arene or calix[8]arene, preferably, the repetition number of the methylene phenol unit in the calixarene is n=1, that is, the repeating structural unit calixarene is calix[4]arene.
4. A method for synthesizing a cross-linked polymer as claimed in claims 1 to 3, characterized in that: The following steps are included: A) preparing nitrocalixarene, comprising: (A1) weighing tert-butylcalixarene monomer and anhydrous organic solvent to prepare a mixed solution with a molar ratio of 1:3 to 5; (A2) adding 1 to 3 times the amount of glacial acetic acid and 4 to 10 times the amount of fuming nitric acid in the amount of the tert-butylcalixarene monomer, mixing evenly, and reacting at 0° C. to 50° C. for 2 h to 8 h; After the reaction (A3) is completed, the mixture is allowed to stand for clarification, and the phases are separated. The upper organic phase is evaporated in vacuo to obtain a solid precipitate, which is washed with an anhydrous organic solvent corresponding to A1 until the washing liquid is neutral to obtain nitrocalixarene, whose chemical structure is: B) preparing aminocalixarene, comprising: (B1) weighing the nitrocalixarene described in step A and an anhydrous organic solvent to prepare a mixed solution with a molar ratio of 1:3 to 6; (B2) adding a palladium-carbon catalyst to the reaction system under a saturated nitrogen atmosphere with a water-oxygen concentration of less than 10 ppm; (B3) firstly introducing hydrogen to replace the original nitrogen atmosphere, and then using a circulating ventilation device to continuously introduce hydrogen to carry out a hydrogenation reduction reaction, maintaining 20°C to 50°C for 20.0h to 48.0h; (B4) After the reaction is completed, water is first injected to terminate the catalytic reaction of the palladium-carbon catalyst, and then the upper organic phase is taken and allowed to stand for phase separation and evaporated in vacuum to obtain aminocalixarene, whose chemical structure is: C) preparing a crosslinked polymer of calixarene, comprising: (C1) weighing the aminocalixarene described in step B and mixing it with an anhydrous solvent to prepare a mixed solution with a molar ratio of 1:3 to 6; (C2) adding a cross-linking agent in an amount of 1 / 8 to 1 / 6 of the aminocalixarene substance and mixing evenly; (C3) adding a condensation aid in an amount of 1 / 10 to 1 / 7 of the aminocalix aromatic substance to carry out a condensation polymerization reaction, maintaining a temperature of 60° C. to 100° C. for 48.0 h to 96 h; (C4) After the reaction is completed, the solid product is obtained by liquid-solid separation, and the solid product is washed more than 3 times with the corresponding anhydrous solvent in step C1, and the solid product is separated by liquid-solid separation, and dried at 60° C. to obtain the cross-linked polymer based on calixarene according to claims 1 to 3.
5. The synthesis method according to claim 4, characterized in that The anhydrous organic solvent includes benzene, toluene, dichloromethane and chloroform.
6. The synthesis method according to claim 4, characterized in that In step A, the tert-butylcalixarene monomer includes tert-butylcalix[4]arene, tert-butylcalix[6]arene and tert-butylcalix[8]arene, and the general chemical structure thereof is: Here, n is the number of repetitions of the methylene phenol unit in the calixarene.
7. The synthesis method according to claim 4, characterized in that In step B, the palladium-carbon catalyst is a palladium-carbon catalyst with an effective substance mass percentage of 5% and water added to a mass percentage of 50%.
8. The synthesis method according to claim 4, wherein in step C, the cross-linking agent comprises 1,3-dichloropropane, 2,2-dichloroethyl ether, 1,4-dichlorobenzene and 2,4-dichloro-1,3,5-triazine, and the condensation auxiliary agent comprises sodium bicarbonate, sodium carbonate, sodium hydroxide and triethylamine.
9. An application based on calixarene cross-linked polymer, characterized in that: The calixarene-based cross-linked polymers described in the aforementioned claims 1 to 3 and the calixarene-based cross-linked polymers obtained by the synthesis methods of claims 4 to 8 are used to separate and enrich lithium ions in salt lake brine.
Citation Information
Cited By
Silicon-based adsorbent for oil gas recovery and preparation method thereof
CN120169326A