Flame-retardant rubber and preparation method thereof

By compounding natural rubber and butadiene rubber and using modified graphene oxide, a three-dimensional cross-linked network structure is formed, which solves the problem of flame retardant migration in rubber and achieves stability of flame retardant performance and maintenance of appearance.

CN118978751AInactive Publication Date: 2024-11-19DONGGUAN XINGQICHEN INTELLIGENT TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411278738.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In flame-retardant rubber, the added flame retardants are prone to migration during processing or use, resulting in a white hazy substance appearing on the product surface, affecting the appearance and reducing the flame-retardant performance.

Method used

It uses a blend of natural rubber and butadiene rubber, and adds modified graphene oxide and organophosphorus flame retardants. By forming a three-dimensional cross-linked network structure, the flame retardants are physically confined, reducing their migration.

Benefits of technology

It effectively prevents uneven migration of flame retardants during product use, maintains stable flame retardant performance, avoids localized decline in flame retardant effect, and improves the overall physical structural stability of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005041000290000081
    Figure BDA0005041000290000081
  • Figure BDA0005041000290000091
    Figure BDA0005041000290000091
Patent Text Reader

Abstract

The invention belongs to the technical field of rubber materials. The invention relates to the field of rubber, in particular to flame-retardant rubber and a preparation method thereof. The product prepared by the invention comprises natural rubber, butadiene rubber and an organophosphorus flame retardant; wherein the mass ratio of the natural rubber to the butadiene rubber is (3.0-3.5): 1; the dosage of the organophosphorus flame retardant is 20-25% of the mass of the natural rubber; the number-average molecular weight of the natural rubber is 25.5 * 10 < 4 > to 32.0 * 10 < 4 >; the number-average molecular weight of the butadiene rubber is 120.0 * 10 < 4 > to 135.0 * 10 < 4 >; the organophosphorus flame retardant comprises a phosphonate flame retardant. The modified graphene oxide accounts for 4-6% of the mass of the natural rubber; the modified graphene oxide is obtained by embedding octadecylamine between graphene oxide layers, and the D50 of the modified graphene oxide is 80-90 nm; in addition, the particle size distribution range of the modified graphene oxide is 10 to 200nm.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of rubber materials, and more specifically, relates to a flame retardant rubber and a preparation method thereof. Background Art

[0002] Flame retardant rubber is a rubber material that has been specially treated or added with flame retardants. It can slow down the burning speed when it encounters fire and reduce the risk of fire spreading. This material is crucial to improve safety, especially in the fields of wires and cables, rubber ropes, conveyor belts, hoses, air ducts, rubber belts, and electronic and electrical industries.

[0003] In order to improve the flame retardant effect of rubber, commonly used methods include:

[0004] Chemical grafting modification of rubber: Phosphorus-nitrogen flame retardants are grafted onto natural rubber by chemical methods to improve compatibility and uniform dispersion. For example, 5-(aminomethyl)-1,3,4-oxadiazole-2-carboxylic acid ethyl ester and triethylamine are reacted with phenylphosphonic dichloride to prepare a reactive flame retardant, which is then added to natural rubber for mixing and vulcanization. This method can improve the flame retardant properties of rubber while maintaining good mechanical properties;

[0005] Blending modification of rubber: Blending rubber with flame-retardant polymers, such as polyvinyl chloride, chlorinated polyethylene, etc., to improve the flame retardancy of rubber. At the same time, adding organic halogen flame retardants and inorganic flame retardants such as antimony trioxide, and inorganic fillers such as aluminum hydroxide to blend with rubber to improve the flame retardancy of rubber;

[0006] In terms of the common blending modification method, the added organic flame retardant is prone to migration under certain temperature and time conditions, resulting in the appearance of white mist on the product surface, which not only affects the appearance of the product, but also easily leads to a significant decrease in its flame retardant properties. Summary of the invention

[0007] The technical problem to be solved by the present invention is that in a flame retardant rubber system, the added flame retardant is prone to migration during processing or use, resulting in the appearance of white misty substances on the surface of the product, which not only affects the appearance of the product but also easily leads to a significant decrease in its flame retardant performance. The present invention provides a flame retardant rubber and a preparation method thereof.

[0008] The object of the present invention is to provide a flame retardant rubber.

[0009] Another object of the present invention is to provide a method for preparing the flame retardant rubber.

[0010] The above-mentioned purpose of the present invention is achieved through the following technical solutions:

[0011] A flame retardant rubber comprising natural rubber, butadiene rubber and an organic phosphorus flame retardant;

[0012] Wherein, the mass ratio of the natural rubber to the butadiene rubber is (3.0-3.5):1;

[0013] The amount of the organophosphorus flame retardant is 20-25% of the mass of the natural rubber;

[0014] The number average molecular weight of the natural rubber is 25.5×10 4 -32.0×10 4 ;

[0015] The number average molecular weight of the butadiene rubber is 120.0×10 4 -135.0×10 4 ;

[0016] The organic phosphorus flame retardant includes a phosphonate flame retardant.

[0017] Furthermore, the phosphonate flame retardant is selected from any one of tris(2-chloroethyl) phosphate, tris(2-chloropropyl) phosphate, tris(1,3-dichloroisopropyl) phosphate, resorcinol bis(diphenyl phosphate), bisphenol A bis(diphenyl phosphate), dimethyl methylphosphonate, and diethyl ethyl phosphate.

[0018] Further, it also includes 4-6% of the mass of natural rubber modified graphene oxide;

[0019] The modified graphene oxide is obtained by embedding octadecylamine between graphene oxide layers.

[0020] Further, by introducing graphene oxide into the rubber system, its layered structure can play a certain lubricating role in the rubber material processing and molding process, thereby facilitating the uniform mixing of the components, and by embedding octadecylamine, its compatibility with both natural rubber and butadiene rubber systems can be effectively improved, thereby avoiding phase separation; more importantly, its layered structure can be dispersed and interspersed in the three-dimensional cross-linked network system of rubber, thereby forming a barrier for the diffusion of organophosphorus flame retardants inside, effectively extending the diffusion path of the flame retardant, thereby further improving the flame retardant effect of the product;

[0021] In addition, when the temperature continues to rise and it is needed to exert its flame retardant effect, after the rubber softens, graphene oxide, due to its light weight, can cooperate with the flame retardant to diffuse quickly to the rubber surface, thus forming an air barrier layer.

[0022] Further, the D50 of the modified graphene oxide is 80-90nm;

[0023] Moreover, the particle size distribution range of the modified graphene oxide is 10-200 nm.

[0024] Graphene oxide with a relatively wide particle size distribution range is selected. When dispersed in the rubber system, it can form a more complex barrier. In particular, large particles and small particles can fill each other, thereby further extending the diffusion path of the flame retardant and reducing the probability of its migration.

[0025] Furthermore, the flame retardant rubber also includes the following raw materials:

[0026] An accelerator accounting for 3-5% of the mass of the natural rubber;

[0027] The accelerator is selected from any one of accelerator M, accelerator DM and accelerator D;

[0028] 1-3% of the natural rubber mass by weight of an antioxidant;

[0029] The antioxidant is selected from any one of antioxidant D and antioxidant 4010;

[0030] 2-4% plasticizer by weight of the natural rubber;

[0031] The plasticizer is selected from any one of aromatic oil, naphthenic oil and paraffin oil;

[0032] 5-7% of the mass of the natural rubber by weight of a vulcanizing agent;

[0033] The vulcanizing agent is prepared by mixing benzoyl peroxide and dinitrosobenzene in a mass ratio of 2:1.

[0034] Furthermore, the polydispersity index of the natural rubber is 2.0-2.2.

[0035] Furthermore, the polydispersity index of the butadiene rubber is 2.0-2.5.

[0036] A method for preparing flame retardant rubber, the specific preparation steps comprising:

[0037] After mixing graphene oxide and water, ultrasonically disperse them for 40-60 minutes at an ultrasonic frequency of 180-200 kHz to obtain a graphene oxide dispersion;

[0038] Dissolve octadecylamine in anhydrous ethanol, add 1-3% of boron trifluoride by weight of octadecylamine, and stir for activation for 30-45 minutes to obtain an ethanol solution of octadecylamine;

[0039] Under the protection of inert gas, an ethanol solution of octadecylamine is added dropwise to the graphene oxide dispersion, and the mixture is heated and stirred for 4-6 hours at a temperature of 68-75° C. and a stirring speed of 300-500 r / min, and then filtered, washed and dried to obtain modified graphene oxide;

[0040] Weigh each component according to the raw material composition;

[0041] Firstly, natural rubber and butadiene rubber are mixed, and then organic phosphorus flame retardant, accelerator, antioxidant, plasticizer and vulcanizer are added. After mixing evenly, the mixture is calendered and then vulcanized to obtain flame retardant rubber.

[0042] Furthermore, in the graphene oxide dispersion, the mass ratio of the graphene oxide to the water is 1:(8.5-9.0); in the ethanol solution of octadecylamine, the mass ratio of the octadecylamine to the anhydrous ethanol is 1:(10-12); and the amount of the ethanol solution of octadecylamine used is 0.15-0.22 times the mass of the graphene oxide dispersion.

[0043] Beneficial technical effects:

[0044] (1) The technical solution of the present invention selects a compound of natural rubber and butadiene rubber as the rubber system, so as to utilize the mutually interlaced three-dimensional network structure formed during the vulcanization process of natural rubber and butadiene rubber, thereby effectively physically confining the organic phosphorus flame retardant molecules in its network structure, increasing its diffusion resistance, and preventing its overflow during the use of the product; in particular, the mixed system of the two rubbers, by using a natural rubber with a small molecular weight and a butadiene rubber with a relatively large molecular weight to compound at a corresponding mass ratio, the natural rubber with a small molecular weight is more easily vulcanized and has a faster vulcanization rate than the butadiene rubber with a larger molecular weight, so that in the processing process, the natural rubber can be preferentially vulcanized faster. The cross-linked network structure is formed quickly, and each component in the system is quickly and evenly confined in its network structure during the processing. The formation of the rapid cross-linked network structure can effectively avoid the uneven migration of components caused by high temperature during the vulcanization process, especially the uneven migration of organophosphorus flame retardants, thereby avoiding the uneven distribution of flame retardants caused during the processing as much as possible; on this basis, butadiene rubber with a larger molecular weight is selected to provide more cross-linking sites, thereby increasing the cross-linking density, and at the same time forming a three-dimensional cross-linked network system interlaced with natural rubber, so that the overall physical structure of the product is stable and reliable. The formation of this network structure can also reduce the migration of organophosphorus flame retardants during the use of the product;

[0045] (2) By selecting natural rubber with a narrower molecular weight distribution range, a narrower molecular weight distribution range can form a more uniform network structure. Moreover, due to the lower molecular weight, natural rubber can form a cross-linked network faster than butadiene rubber. Therefore, under the induction of the uniform cross-linked network, butadiene rubber also tends to form a relatively uniform structure when forming an interpenetrating network structure during the cross-linking process. Therefore, the migration of local flame retardant molecules caused by local structural inhomogeneity can be avoided, thereby causing a rapid decrease in overall flame retardant performance due to a decrease or failure of the local flame retardant effect. DETAILED DESCRIPTION

[0046] The present invention is further described below with reference to specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0047] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.

[0048] Example 1

[0049] After mixing graphene oxide and water, ultrasonic dispersion is performed for 40 minutes at an ultrasonic frequency of 180 kHz to obtain a graphene oxide dispersion;

[0050] The mass ratio of the graphene oxide to the water is 1:8.5;

[0051] Dissolve octadecylamine in anhydrous ethanol, add 1% of boron trifluoride by mass of octadecylamine, and stir with a stirrer at a speed of 200 r / min for 30 minutes to obtain an ethanol solution of octadecylamine;

[0052] The mass ratio of the octadecylamine to the anhydrous ethanol is 1:10;

[0053] Under argon gas protection, add octadecylamine ethanol solution to the graphene oxide dispersion, control the drop rate to 10 mL / min, heat and stir for 4 h at 68° C. and 300 r / min, filter, wash and dry, and then sieve to obtain modified graphene oxide;

[0054] The modified graphene oxide obtained by screening has a D50 of 80 nm and a particle size distribution range of 10-200 nm;

[0055] The amount of the ethanol solution of octadecylamine used is 0.15 times the mass of the graphene oxide dispersion;

[0056] Weigh the components according to the following raw material composition:

[0057] Prepare natural rubber and butadiene rubber in a mass ratio of 3.0:1;

[0058] The number average molecular weight of the natural rubber is 25.5×10 4 ;

[0059] The number average molecular weight of the butadiene rubber is 120.0×10 4 ;

[0060] The polydispersity index of the natural rubber is 2.0;

[0061] The polydispersity index of the butadiene rubber is 2.0;

[0062] Prepare 20% of the mass of the natural rubber organophosphorus flame retardant; the organophosphorus flame retardant is a phosphonate flame retardant;

[0063] The phosphonate flame retardant is selected from tris(2-chloroethyl) phosphate;

[0064] Preparing 4% of the mass of the natural rubber modified graphene oxide;

[0065] Prepare an accelerator with a mass percentage of 3% of the natural rubber;

[0066] The accelerator is selected from accelerator M;

[0067] Prepare an antioxidant with a mass percentage of 1% of the natural rubber;

[0068] The antioxidant is selected from antioxidant D;

[0069] Prepare 2% plasticizer by mass of the natural rubber;

[0070] The plasticizer is selected from aromatic oils;

[0071] Prepare a vulcanizing agent with a mass percentage of 5% of the natural rubber;

[0072] The vulcanizing agent is a mixture of benzoyl peroxide and dinitrosobenzene in a mass ratio of 2:1;

[0073] First, natural rubber and butadiene rubber are mixed, and then organic phosphorus flame retardant, accelerator, antioxidant, plasticizer and vulcanizer are added. After mixing evenly, calendering is performed, and hot pressing and vulcanization are performed for 8 minutes at a temperature of 150°C and a pressure of 12MPa to obtain flame retardant rubber.

[0074] Example 2

[0075] After mixing graphene oxide and water, ultrasonic dispersion is performed for 40 minutes at an ultrasonic frequency of 190 kHz to obtain a graphene oxide dispersion;

[0076] The mass ratio of the graphene oxide to the water is 1:8.8;

[0077] Dissolve octadecylamine in anhydrous ethanol, add 2% of boron trifluoride by weight of octadecylamine, and stir with a stirrer at 200 r / min for 35 minutes to obtain an ethanol solution of octadecylamine;

[0078] The mass ratio of the octadecylamine to the anhydrous ethanol is 1:11;

[0079] Under argon gas protection, add octadecylamine ethanol solution to the graphene oxide dispersion, control the drop rate to 10 mL / min, heat and stir at 72° C., stir at 400 r / min, react for 5 h, filter, wash and dry, and then sieve to obtain modified graphene oxide;

[0080] The modified graphene oxide obtained by screening has a D50 of 85 nm and a particle size distribution range of 10-200 nm;

[0081] The amount of the ethanol solution of octadecylamine used is 0.18 times the mass of the graphene oxide dispersion;

[0082] Weigh the components according to the following raw material composition:

[0083] Prepare natural rubber and butadiene rubber in a mass ratio of 3.2:1;

[0084] The number average molecular weight of the natural rubber is 28.0×10 4 ;

[0085] The number average molecular weight of the butadiene rubber is 122.0×10 4 ;

[0086] The polydispersity index of the natural rubber is 2.1;

[0087] The polydispersity index of the butadiene rubber is 2.2;

[0088] Prepare 22% of the mass of the natural rubber organophosphorus flame retardant; the organophosphorus flame retardant is a phosphonate flame retardant;

[0089] The phosphonate flame retardant is selected from tris(2-chloropropyl) phosphate;

[0090] Preparing 5% of the mass of the natural rubber modified graphene oxide;

[0091] Prepare an accelerator with a mass percentage of 4% of the natural rubber;

[0092] The accelerator is selected from accelerator DM;

[0093] Prepare an antioxidant with a mass percentage of 2% of the natural rubber;

[0094] The antioxidant is selected from antioxidant 4010;

[0095] Prepare 3% plasticizer by mass of the natural rubber;

[0096] The plasticizer is selected from naphthenic oil;

[0097] Prepare a vulcanizing agent with a mass percentage of 6% of the natural rubber;

[0098] The vulcanizing agent is a mixture of benzoyl peroxide and dinitrosobenzene in a mass ratio of 2:1;

[0099] First, natural rubber and butadiene rubber are mixed, and then organic phosphorus flame retardant, accelerator, antioxidant, plasticizer and vulcanizer are added. After mixing evenly, calendering is performed, and hot pressing and vulcanization are performed for 9 minutes at a temperature of 152°C and a pressure of 13MPa to obtain flame retardant rubber.

[0100] Example 3

[0101] After mixing graphene oxide and water, ultrasonic dispersion is performed for 60 minutes at an ultrasonic frequency of 200 kHz to obtain a graphene oxide dispersion;

[0102] The mass ratio of the graphene oxide to the water is 1:9.0;

[0103] Dissolve octadecylamine in anhydrous ethanol, add 3% of boron trifluoride by weight of octadecylamine, and stir with a stirrer at a speed of 200 r / min for 45 minutes to obtain an ethanol solution of octadecylamine;

[0104] The mass ratio of the octadecylamine to the anhydrous ethanol is 1:12;

[0105] Under argon gas protection, add octadecylamine ethanol solution to the graphene oxide dispersion, control the drop rate to 10 mL / min, heat and stir for 6 h at 75° C. and 500 r / min, filter, wash and dry, and then sieve to obtain modified graphene oxide;

[0106] The modified graphene oxide obtained by screening has a D50 of 90 nm and a particle size distribution range of 10-200 nm;

[0107] The amount of the ethanol solution of octadecylamine used is 0.22 times the mass of the graphene oxide dispersion;

[0108] Weigh the components according to the following raw material composition:

[0109] Prepare natural rubber and butadiene rubber in a mass ratio of 3.5:1;

[0110] The number average molecular weight of the natural rubber is 32.0×10 4 ;

[0111] The number average molecular weight of the butadiene rubber is 135.0×10 4 ;

[0112] The polydispersity index of the natural rubber is 2.2;

[0113] The polydispersity index of the butadiene rubber is 2.5;

[0114] Prepare 25% of the mass of the natural rubber organophosphorus flame retardant; the organophosphorus flame retardant is a phosphonate flame retardant;

[0115] The phosphonate flame retardant is selected from resorcinol bis(diphenyl phosphate);

[0116] Preparing 6% of the mass of the natural rubber modified graphene oxide;

[0117] Prepare an accelerator with a mass percentage of 5% of the natural rubber;

[0118] The accelerator is selected from accelerator D;

[0119] Prepare an antioxidant with a mass percentage of 3% of the natural rubber;

[0120] The antioxidant is selected from antioxidant 4010;

[0121] Prepare 4% plasticizer by mass of the natural rubber;

[0122] The plasticizer is selected from paraffin oil;

[0123] Prepare a vulcanizing agent with a mass percentage of 7% of the natural rubber;

[0124] The vulcanizing agent is a mixture of benzoyl peroxide and dinitrosobenzene in a mass ratio of 2:1;

[0125] First, natural rubber and butadiene rubber are mixed, and then organic phosphorus flame retardant, accelerator, antioxidant, plasticizer and vulcanizer are added. After mixing evenly, calendering is performed, and hot pressing and vulcanization are performed for 10 minutes at a temperature of 155°C and a pressure of 15MPa to obtain flame retardant rubber.

[0126] Example 4

[0127] Compared with Example 1, this embodiment is different in that:

[0128] The polydispersity index of the natural rubber is 2.4;

[0129] The polydispersity index of the butadiene rubber is 2.6;

[0130] The rest of the conditions remain unchanged.

[0131] Example 5

[0132] Compared with Example 1, this embodiment is different in that:

[0133] No octadecylamine was added and the other conditions remained unchanged.

[0134] Example 6

[0135] Compared with Example 1, this embodiment is different in that:

[0136] No modified graphene oxide was added, and the other conditions remained unchanged.

[0137] Comparative Example 1

[0138] The difference between this comparative example and Example 1 is that natural rubber of equal mass is used to replace butadiene rubber, that is, butadiene rubber is not added, and other conditions remain unchanged.

[0139] Comparative Example 2

[0140] The difference between this comparative example and Example 1 is that an equal mass of butadiene rubber is used to replace natural rubber, that is, no natural rubber is added, and other conditions remain unchanged.

[0141] Comparative Example 3

[0142] Compared with Example 1, this comparative example has the following differences:

[0143] The number average molecular weight of the natural rubber is 125.5×10 4 ; The rest of the conditions remain unchanged.

[0144] The performance tests were performed on the products obtained in the examples and comparative examples. The specific test methods and test results are as follows:

[0145] The flame retardant grade test was carried out according to GB / T10707-2008, the sample size was 120mm×12.5mm×4.0mm, the laboratory temperature was (25±2)℃, the relative humidity was (50±5)%, and the absorbent cotton was laid under the sample during the test. The absorbent cotton size was 50mm×50mm×5mm, and the flame retardant grade was 1. The detailed test results are shown in Table 1;

[0146] The same test method as above was used, except that the samples of each embodiment and comparative example were placed at a temperature of 60° C. and a relative humidity of 70% for 30 days before being subjected to the above test to obtain a flame retardancy grade of 2. The detailed test results are shown in Table 1.

[0147] The tensile properties were tested according to GB / T528-2009, and the detailed test results are shown in Table 1;

[0148] Table 1: Product performance test results

[0149]

[0150]

[0151] It can be seen from the test results in Table 1 that the product obtained by the present invention has excellent mechanical properties and good flame retardant properties. After long-term high-temperature and high-humidity aging treatment, the flame retardant properties can also be effectively maintained.

[0152] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A flame retardant rubber, characterized in that: Including natural rubber, butadiene rubber and organophosphorus flame retardants; Wherein, the mass ratio of the natural rubber to the butadiene rubber is (3.0-3.5):1; The amount of the organophosphorus flame retardant is 20-25% of the mass of the natural rubber; The number average molecular weight of the natural rubber is 25.5×10 4 -32.0×10 4 ; The number average molecular weight of the butadiene rubber is 120.0×10 4 -135.0×10 4 ; The organic phosphorus flame retardant includes a phosphonate flame retardant.

2. The flame retardant rubber according to claim 1, characterized in that: The phosphonate flame retardant is selected from any one of tris(2-chloroethyl) phosphate, tris(2-chloropropyl) phosphate, tris(1,3-dichloroisopropyl) phosphate, resorcinol bis(diphenyl phosphate), bisphenol A bis(diphenyl phosphate), dimethyl methylphosphonate, and diethyl ethyl phosphate.

3. The flame retardant rubber according to claim 1, characterized in that: Also included is modified graphene oxide at 4-6% by mass of natural rubber; The modified graphene oxide is obtained by embedding octadecylamine between graphene oxide layers.

4. The flame retardant rubber according to claim 3, characterized in that: The D50 of the modified graphene oxide is 80-90nm; Moreover, the particle size distribution range of the modified graphene oxide is 10-200 nm.

5. The flame retardant rubber according to claim 1, characterized in that: The flame retardant rubber also includes the following raw materials: An accelerator accounting for 3-5% of the mass of the natural rubber; The accelerator is selected from any one of accelerator M, accelerator DM and accelerator D; 1-3% of the natural rubber mass by weight of an antioxidant; The antioxidant is selected from any one of antioxidant D and antioxidant 4010; 2-4% plasticizer by weight of the natural rubber; The plasticizer is selected from any one of aromatic oil, naphthenic oil and paraffin oil; 5-7% of the mass of the natural rubber by weight of a vulcanizing agent; The vulcanizing agent is prepared by mixing benzoyl peroxide and dinitrosobenzene in a mass ratio of 2:

1.

6. The flame retardant rubber according to claim 1, characterized in that: The polydispersity index of the natural rubber is 2.0-2.

2.

7. The flame retardant rubber according to claim 1, characterized in that: The polydispersity index of the butadiene rubber is 2.0-2.

5.

8. A method for preparing the flame retardant rubber according to any one of claims 1 to 7, characterized in that: The specific preparation steps include: After mixing graphene oxide and water, ultrasonically disperse them for 40-60 minutes at an ultrasonic frequency of 180-200 kHz to obtain a graphene oxide dispersion; Dissolve octadecylamine in anhydrous ethanol, add 1-3% of boron trifluoride by weight of octadecylamine, and stir for activation for 30-45 minutes to obtain an ethanol solution of octadecylamine; Under the protection of inert gas, an ethanol solution of octadecylamine is added dropwise to the graphene oxide dispersion, and the mixture is heated and stirred for 4-6 hours at a temperature of 68-75° C. and a stirring speed of 300-500 r / min, and then filtered, washed and dried to obtain modified graphene oxide; Weigh each component according to the raw material composition; Firstly, natural rubber and butadiene rubber are mixed, and then organic phosphorus flame retardant, accelerator, antioxidant, plasticizer and vulcanizer are added. After mixing evenly, the mixture is calendered and then vulcanized to obtain flame retardant rubber.

9. The method for preparing a flame retardant rubber according to claim 8, characterized in that: In the graphene oxide dispersion, the mass ratio of the graphene oxide to the water is 1:(8.5-9.0); in the ethanol solution of octadecylamine, the mass ratio of the octadecylamine to the anhydrous ethanol is 1:(10-12); and the amount of the ethanol solution of octadecylamine used is 0.15-0.22 times the mass of the graphene oxide dispersion.

Citation Information

Patent Citations

  • Polymer-base flame-proof composite material

    CN101121796A

  • Flame-retardant protective coating for rubber and plastic products and preparation method thereof

    CN110128918A

  • High-wear-resistance graphene modified natural rubber and preparation method thereof

    CN115073826A

Cited By

  • Bending-resistant flame-retardant rubber, preparation method thereof and new energy cable containing bending-resistant flame-retardant rubber

    CN121136225A