Foam molded body

By adding fibrous fillers and foaming agents to the resin, a multi-layered foamed molded body is formed, which solves the problem of insufficient mechanical strength of general plastics and achieves high strength, lightweight and impact resistance, making it suitable for industrial products that can replace engineering plastics or metal materials.

CN118978763APending Publication Date: 2024-11-19PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411046325.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2019-02-08
Filing Date
2020-02-05
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

General-purpose plastics have insufficient mechanical strength, which limits their application in mechanical products such as automobiles and electrical/electronic/information products. Engineering plastics, on the other hand, are expensive, difficult to recycle, and have a high environmental impact.

Method used

By adding 15-80% by mass of fibrous filler and 0.01-10% by mass of foaming agent to resin, a multi-layered foamed molded body is formed, including a skin layer, a core surface layer, and a core inner layer. The aspect ratio of the fibrous filler and the cell diameter of the foaming agent are controlled to improve mechanical strength and reduce weight.

Benefits of technology

It achieves high-strength, lightweight foamed molded bodies with good impact resistance and appearance, and can replace engineering plastics or metal materials to reduce the manufacturing cost of industrial products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978763A_ABST
    Figure CN118978763A_ABST
Patent Text Reader

Abstract

A foam molded body according to the present invention contains a base resin, 15-80% by mass (inclusive) of a filler, and 0.01-10% by mass (inclusive) of a foaming agent, the foaming agent having a foaming ratio of 1.1 times or more.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application of an application with a filing date of February 5, 2020, application number 202010081130.8, and invention name “Foamed Molded Body”. Technical Field

[0002] The present invention relates to a composite resin composition capable of realizing a foamed molded product having excellent mechanical properties. Background Art

[0003] So-called "general-purpose plastics" such as polyethylene (PE), polypropylene (PP), polystyrene (PS), and polyvinyl chloride (PVC) are not only very cheap, but also easy to shape, and are light at a fraction of the weight of metals or ceramics. Therefore, general-purpose plastics are often used as materials for a variety of daily necessities such as bags, various packages, various containers, and sheets. In addition, they are used as materials for industrial parts such as automobile parts and electrical parts, as well as daily necessities and sundry goods.

[0004] However, general-purpose plastics have disadvantages such as insufficient mechanical strength. Therefore, general-purpose plastics do not have sufficient properties required for materials used in various industrial products such as mechanical products such as automobiles and electrical / electronic / information products, and their application range is currently limited.

[0005] On the other hand, so-called "engineering plastics" such as polycarbonate, fluororesin, acrylic resin, and polyamide have excellent mechanical properties and are used in various industrial products such as mechanical products such as automobiles and electrical / electronic / information products. However, engineering plastics have problems such as high prices, difficulty in monomer recycling, and high environmental load.

[0006] Therefore, it is expected to significantly improve the material properties (mechanical strength, etc.) of general-purpose plastics. In order to strengthen general-purpose plastics, it is known that a technique is used to improve the mechanical strength of general-purpose plastics by dispersing natural fibers, glass fibers, carbon fibers, etc. as fibrous fillers in the resin of general-purpose plastics. Among them, organic fibrous fillers such as cellulose are inexpensive and have excellent environmental friendliness when discarded, and therefore have attracted attention as reinforcing fibers.

[0007] Furthermore, as a plastic that achieves weight reduction while taking advantage of the above-mentioned characteristics, a foamed molded article obtained by adding a foaming agent to a resin and foam-molding the resin has been proposed.

[0008] For example, in Patent Document 1, a composite resin having a low concentration of cellulose fibers uniformly dispersed in a polyamide resin is foamed to improve surface appearance and impact resistance.

[0009] Prior art literature

[0010] Patent Literature

[0011] Patent Document 1: Japanese Patent No. 6351574 Summary of the invention

[0012] The foamed molded article of the present invention comprises a main resin, 15% to 80% by mass of a filler, and 0.01% to 10% by mass of a foaming agent, wherein the foaming agent provides a foaming ratio of 1.1 times or more. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] Figure 1 It is a schematic diagram which shows the structure of the foamed molded article which concerns on embodiment of this invention.

[0014] Figure 2 This is a schematic diagram for explaining a filler according to an embodiment.

[0015] Figure 3 This is a schematic diagram for explaining a skin layer, a core surface layer, and a core internal layer of a foamed molded body according to an embodiment.

[0016] Figure 4 It is a flowchart of the manufacturing method of the foaming molded article which concerns on embodiment.

[0017] Figure 5 It is a figure which shows the result of the Example and the comparative example in embodiment.

[0018] Description of Reference Numerals

[0019] 1 Main agent resin

[0020] 2Fiber filler

[0021] 3 bubble holes

[0022] 4 Cortex

[0023] 5 core surface

[0024] 6-core inner layer

[0025] 10 Foamed body DETAILED DESCRIPTION

[0026] In Patent Document 1, cellulose fibers as fibrous fillers are uniformly dispersed to improve impact resistance. However, since the content of cellulose fibers is low, when a resin such as general-purpose plastic is used, impact resistance is insufficient.

[0027] The present invention has been made to solve the above-mentioned conventional problems, and an object of the present invention is to provide a foamed molded product having light weight and impact resistance.

[0028] The foamed molded article of the first aspect comprises a main resin, 15% to 80% by mass of a filler, and 0.01% to 10% by mass of a foaming agent, wherein the foaming agent provides a foaming ratio of 1.1 times or more.

[0029] The foamed molded body of the second aspect is the following foamed molded body: In the foamed molded body of the first aspect, the foamed molded body may have:

[0030] The surface cortex,

[0031] A core surface layer located inside the skin layer and having a mass concentration of the filler lower than that of the skin layer, and

[0032] A core inner layer is located inside the core surface layer and has a lower mass concentration of the filler than the core surface layer.

[0033] In other words, the foamed molded body of the second aspect, in the above-mentioned first aspect, has two skin layers, two core surface layers located between the two skin layers and a core inner layer located between the two core surface layers, the mass concentration of the filler in the core surface layer can be lower than the mass concentration of the filler in the skin layer, and the mass concentration of the filler in the core inner layer can be lower than the mass concentration of the filler in the core surface layer.

[0034] The foaming molded body of the third aspect is the following foaming molded body: in the foaming molded body of the above-mentioned second aspect, the ratio of the mass concentration of the filler in the skin layer to the mass concentration of the filler in the core inner layer can be greater than 1.05, and the ratio of the mass concentration of the filler in the core surface layer to the mass concentration of the filler in the core inner layer can be greater than 1.02.

[0035] The foamed molded body of the fourth aspect is the following foamed molded body: in the foamed molded body of the second aspect or the foamed molded body of the third aspect, the cell diameter of the foaming agent contained in the core surface layer can be smaller than the cell diameter of the foaming agent contained in the core inner layer.

[0036] The foamed molded body of the fifth aspect is the following foamed molded body: in the foamed molded body of the fourth aspect, the pore diameter of the foaming agent contained in the core surface layer can be 40μm~80μm, and the pore diameter of the foaming agent contained in the core inner layer can be 90μm~500μm.

[0037] A foamed molded product according to a sixth aspect is the foamed molded product according to any one of the first to fifth aspects, wherein the filler may include a filler having an aspect ratio of 2 or less and a filler having an aspect ratio of 10 or more.

[0038] A foamed molded product according to a seventh aspect is the foamed molded product according to the sixth aspect, wherein the proportion of a filler having an aspect ratio of 2 or less is greater than the proportion of a filler having an aspect ratio of 10 or more.

[0039] The foaming molded body of the eighth aspect is the following foaming molded body: in the foaming molded body of the above-mentioned seventh aspect, the proportion of fillers with an aspect ratio of less than 2 in the filler can be greater than 50% and less than 70%, and the proportion of fillers with an aspect ratio of greater than 10 in the filler can be greater than 1% and less than 10%.

[0040] Hereinafter, the foamed molded article according to the embodiment of the present invention will be described with reference to the drawings. It should be noted that in the following description, the same reference numerals are attached to the same components, and the description thereof will be appropriately omitted.

[0041] (Implementation Method)

[0042] Figure 1 It is a schematic diagram which shows the structure of the foamed molded article 10 which concerns on embodiment.

[0043] The foamed molded article 10 of the present embodiment includes a main resin 1, 15% to 80% by mass of a filler 2, and 0.01% to 10% by mass of a foaming agent. The foaming agent provides a foaming ratio of 1.1 times or more.

[0044] According to the foamed molded article 10 , since the filler 2 is contained in the mass concentration within the above range and the expansion ratio by the foaming agent is within the above range, high strength and light weight can be achieved.

[0045] Hereinafter, constituent members constituting the foamed molded body 10 will be described.

[0046] <Main resin>

[0047] In the present embodiment, in order to ensure good formability, the main agent resin 1 is preferably a thermoplastic resin. As a thermoplastic resin, olefin resins (including cyclic olefin resins), styrene resins, (meth) acrylic resins, organic acid vinyl ester resins or derivatives thereof, vinyl ether resins, halogen-containing resins, polycarbonate resins, polyester resins, polyamide resins, thermoplastic polyurethane resins, polysulfone resins (polyethersulfone, polysulfone, etc.), polyphenylene ether resins (polymers of 2,6-xylenol, etc.), cellulose derivatives (cellulose esters, cellulose carbamates, cellulose ethers, etc.), silicone resins (polydimethylsiloxane, polymethylphenylsiloxane, etc.), rubber or elastomer (polybutadiene, polyisoprene and other diene rubbers, styrene-butadiene copolymers, acrylonitrile-butadiene copolymers, acrylic rubber, polyurethane rubber, silicone rubber, etc.), etc. The above resins can be used alone or in combination of two or more. It should be noted that the main agent resin 1 is not limited to the above materials as long as it has thermoplasticity.

[0048] Among these thermoplastic resins, the main resin 1 is preferably an olefin resin with a relatively low melting point. As an olefin resin, in addition to the homopolymer of an olefin monomer, it also includes a copolymer of an olefin monomer, a copolymer of an olefin monomer and other copolymerizable monomers. As an olefin monomer, for example, chain olefins (ethylene, propylene, 1-butene, isobutylene, 1-pentene, 4-methyl-1-pentene, 1-octene and other α-C2-20 olefins, etc.), cyclic olefins, etc. can be cited. These olefin monomers can be used alone or in combination of two or more. Among the above-mentioned olefin monomers, chain olefins such as ethylene and propylene are preferred. As other copolymerizable monomers, for example, fatty acid vinyl esters such as vinyl acetate and vinyl propionate; (meth) acrylic acid monomers such as (meth) acrylic acid, alkyl (meth) acrylic acid esters, and glycidyl (meth) acrylic acid; unsaturated dicarboxylic acids or their anhydrides such as maleic acid, fumaric acid, and maleic anhydride; vinyl esters of carboxylic acids (such as vinyl acetate, vinyl propionate, etc.); cyclic olefins such as norbornene and cyclopentadiene; and dienes such as butadiene and isoprene. These copolymerizable monomers can be used alone or in combination of two or more. As specific examples of olefin resins, copolymers of chain olefins (especially α-C2-4 olefins) such as polyethylene (low-density, medium-density, high-density or linear low-density polyethylene, etc.), polypropylene, ethylene-propylene copolymers, ethylene-propylene-butene-1 and other terpolymers can be listed.

[0049] The content of the main component resin 1 in the present embodiment is preferably more than 10 mass % and less than 85 mass %. In addition, more preferably more than 15 mass % and less than 75 mass %, further preferably more than 20 mass % and less than 65 mass %. If the content of the main component resin 1 is less than 10 mass %, the fluidity variation during pellet forming and foam forming occurs, and poor forming occurs. On the other hand, if the content of the main component resin 1 exceeds 85 mass %, then the improvement effect of the foaming molding strength brought by adding fibrous filler 2 cannot be obtained.

[0050] <Dispersant>

[0051] Next, the dispersant is described. In the present embodiment, the dispersant is included in order to improve the adhesion between the fibrous filler 2 and the main resin 1 or the dispersibility of the fibrous filler 2 in the main resin 1. As the dispersant, various titanate coupling agents, silane coupling agents, unsaturated carboxylic acids, maleic acid, maleic anhydride, or modified polyolefins, fatty acids, fatty acid metal salts, fatty acid esters, etc. obtained by grafting the anhydride can be cited. The above-mentioned silane coupling agent is preferably an unsaturated hydrocarbon-based or epoxy-based silane coupling agent. There is no problem even if the surface of the dispersant is treated with a thermosetting or thermoplastic polymer component for modification.

[0052] The content of the dispersant in the present embodiment is preferably more than 0.01 mass % and below 20 mass %, more preferably more than 0.1 mass % and below 10 mass %, further preferably more than 0.5 mass % and below 5 mass %.When the content of dispersant is lower than 0.01 mass %, poor dispersion is produced.On the other hand, when the content of dispersant exceeds 20 mass %, the intensity of foaming molding reduces.Dispersant is suitably selected according to the combination of main component resin 1 and filler 2, and when not needing the combination of dispersant, dispersant can not be added.

[0053] <Fiber-like filler>

[0054] Next, the fibrous filler 2 is described. In the present embodiment, in the foamed molded body 10 molded using the composite resin composition, the fibrous filler 2 (hereinafter sometimes simply referred to as "fiber") is used mainly for the purpose of improving mechanical properties and improving dimensional stability due to a reduction in the linear expansion coefficient. For this purpose, the fibrous filler 2 preferably has a higher elastic modulus than the main resin 1, and specifically can be carbon fiber (Carbonfiber), carbon nanotubes, pulp, cellulose, cellulose nanofiber, wood cellulose, wood cellulose nanofiber, basic magnesium sulfate fiber (basic magnesium sulfate fiber), potassium titanate fiber, aluminum borate fiber, calcium silicate fiber, calcium carbonate fiber, silicon carbide fiber, wollastonite, hard calcium silicate, various metal fibers, natural fibers such as cotton, silk, wool or hemp, jute fiber, regenerated fibers such as rayon or cuprammonium fiber, semi-synthetic fibers such as acetate fiber and Promix, synthetic fibers such as polyester, polyacrylonitrile, polyamide, aramid, polyolefin, and modified fibers chemically modified on their surfaces and ends. In addition, further, among them, from the viewpoint of availability, high elastic modulus, and low linear expansion coefficient, carbon and cellulose are particularly preferred. And from the viewpoint of environmental protection, natural fibers of cellulose are preferred.

[0055] The content (mass concentration) of the fibrous filler 2 in the present embodiment is preferably more than 15 mass % and below 85 mass %. In addition, more preferably more than 20 mass % and below 80 mass %, further preferably more than 30 mass % and below 70 mass %. When the content (mass concentration) of the fibrous filler 2 is less than 15 mass %, the improvement effect of the intensity of the foaming molded body 10 brought by the addition of the fibrous filler 2 cannot be obtained. On the other hand, if the content (mass concentration) of the fibrous filler 2 exceeds 85 mass %, the fluidity variation during pellet forming and foam forming occurs, and poor forming occurs.

[0056] Figure 2 FIG. 2 is a schematic diagram for explaining a filler 2 according to an embodiment. The shape of the fibrous filler 2 is explained. Figure 2As shown, symbol L is the length of the fibrous filler 2 (hereinafter, sometimes referred to as "fiber length"), and symbol d is the width of the fibrous filler 2 (hereinafter, sometimes referred to as "fiber diameter"). The fibrous filler 2 is preferably a mixed fiber of fiber 2A with a large aspect ratio (L / d) and fiber 2B with a small aspect ratio (L / d). If there are more fibers 2A with a large aspect ratio, the elastic modulus increases. The aspect ratio of the fibrous filler 2A is preferably greater than 10. However, if there are more fibers 2A with a large aspect ratio, the impact resistance deteriorates. In addition, the fiber agglomerates increase and the appearance deteriorates. On the other hand, if there are more fibers 2B with a small aspect ratio, the impact resistance improves, the fiber agglomerates are less, and the appearance is also good. The aspect ratio of the fibrous filler 2B is preferably less than 2. However, if there are more fibers 2B with a small aspect ratio, the elastic modulus decreases.

[0057] The relation of aspect ratio and elastic modulus is described.When foaming molding 10 is applied stress load, if there is the fiber 2A with large aspect ratio, even if fiber elongation, the fiber with high rigidity is also difficult to elongate, therefore, can not be out of shape as foaming molding 10.Therefore, elastic modulus improves.On the other hand, under the situation of the fiber 2B with little aspect ratio, when stress load, the deformation suppression effect that fiber brings weakens, and is out of shape as foaming molding 10, and elastic modulus reduces.

[0058] The aspect ratio and impact resistance are described. When the foaming molded body 10 is subjected to an impact load, if there is a fiber 2A with a large aspect ratio, the fiber cannot follow the elongation of the resin, and cracks are generated between the resin and the fiber, which develops into a break. On the other hand, in the case of the fiber 2B with a small aspect ratio, since the fiber is thin, the fiber follows the elongation of the resin during the impact load, and it is difficult to generate cracks and is not easy to break.

[0059] The relationship between the aspect ratio and the appearance is described. By simultaneously mixing the fiber 2A with a large aspect ratio and the fiber 2B with a small aspect ratio, the fiber 2B with a small aspect ratio is added between the fiber 2A with a large aspect ratio. Agglomeration is suppressed and the appearance is improved.

[0060] As mentioned above, from the viewpoint of elastic modulus, impact resistance, appearance, preferably the fiber 2A with large aspect ratio and the fiber 2B with small aspect ratio are mixed in the foaming molding 10. Can calculate the mixing ratio of each fiber by simulation under what kind of relationship characteristic becomes better. About the proportion of each fiber in the fibrous filler 2, preferably the existence ratio of the fiber 2A with aspect ratio more than 10 is more than 1% and less than 10%, and the existence ratio of the fiber 2B with aspect ratio less than 2 is more than 50% and less than 70%.

[0061] In addition, the existence ratio of other fibers having an aspect ratio of greater than 2 and less than 10 is 20% or more and 49% or less.

[0062] Next, the characteristics of the fibrous filler 2 are described. The types of the main resin 1 and the fibrous filler 2 are as described above. On the other hand, relative to the main resin 1, if the fibrous filler 2 is too soft, that is, the elastic modulus is small, the elastic modulus of the composite resin composition as a whole becomes small, and the strength is reduced as a result. On the other hand, if the fibrous filler 2 is too hard relative to the main resin 1, that is, the elastic modulus is large, the shock wave generated during the impact is not propagated and is absorbed by the interface between the main resin 1 and the fibrous filler 2, therefore, cracks and cracks are easily generated near the interface, and as a result, the impact resistance is reduced. Therefore, the relationship between the elastic modulus of the main resin 1 and the fibrous filler 2 is preferably that the elastic modulus of the fibrous filler 2 is higher, and the difference is as small as possible. The optimal relationship is calculated by the simulation results, and the elastic modulus difference between the main resin 1 and the fibrous filler 2 is preferably within 20GPa.

[0063] In addition, in order to improve the adhesion to the main resin 1 or the dispersibility in the composite resin composition, the fibrous fillers 2 may be surface-treated with various titanate coupling agents, silane coupling agents, unsaturated carboxylic acids, maleic acid, maleic anhydride, or modified polyolefins grafted with the anhydride thereof, fatty acids, fatty acid metal salts, fatty acid esters, etc. Alternatively, fibrous fillers surface-treated with thermosetting or thermoplastic polymer components may be used.

[0064] <Foaming agent>

[0065] Next, the foaming agent is described. In the present embodiment, the foaming agent is used to supply gas for forming bubbles, i.e., foaming holes, during foaming molding. Here, the foaming holes are pores formed by the gas generated by the thermal decomposition of the foaming agent and the gas generated by the solubility change of the dissolved gas in the resin. The foaming agent is roughly divided into chemical foaming agents and physical foaming agents, but there is no particular restriction. As chemical foaming agents, organic chemical foaming agents such as ADCA (azodicarbonamide), DPT (N, N'-dinitrosopentamethylenetetramine), OBSH (4,4'-oxybisbenzenesulfonylhydrazine), bicarbonates such as sodium bicarbonate, carbonates such as sodium carbonate, inorganic chemical foaming agents such as combinations of bicarbonates and organic acid salts such as citrates, etc. can be listed. These chemical foaming agents can be used alone or in combination of two or more, and foaming aids (urea compounds, zinc compounds, etc.) can also be used. Examples of the physical foaming agent include freon gas, hydrocarbon gas, liquefied gases such as nitrogen gas and carbon dioxide gas, and supercritical fluids such as nitrogen gas and carbon dioxide.

[0066] The content of the whipping agent in the present embodiment is preferably more than 0.01 mass % and less than 15 mass %. In addition, more preferably more than 0.1 mass % and less than 10 mass %, further preferably more than 0.5 mass % and less than 5 mass %. If the content of whipping agent is less than 0.01 mass %, then the foaming core reduces, so the foaming cell diameter becomes larger, and the density deviation in the foaming molding 10 becomes larger, and the appearance variation deteriorates. On the other hand, if the content of whipping agent exceeds 15 mass %, then the intensity of the foaming molding 10 reduces.

[0067] Here, the relationship between the structure and impact resistance of the foaming molded body 10 is described. If the elastic modulus of the surface layer of the foaming molded body 10 is high, the rigidity of the foaming molded body 10 as a whole increases, and when the foaming molded body 10 is impact-loaded, the impact can be absorbed inside the foaming molded body 10, and the impact resistance is improved.

[0068] The relationship between the structure of the foamed molded article and the appearance will be described. Since the foamed cells 3 are not present on the surface of the foamed molded article 10, the deterioration of the surface roughness due to the foamed cells 3 is suppressed, and the appearance is improved.

[0069] As described above, from the viewpoint of impact resistance and appearance, the foamed molded article 10 preferably has a layer structure with a high elastic modulus of the surface layer, no foamed cells 3, and the ability to absorb impact inside the foamed molded article 10 and achieve weight reduction.

[0070] Figure 3 1 is a schematic diagram for explaining the skin layer 4, the core surface layer 5 and the core inner layer 6 of the foaming molded body 10 of the embodiment. Figure 3 As shown, the foamed molded body 10 is composed of a skin layer 4, a core surface layer 5, a core inner layer 6, a core surface layer 5 and a skin layer 4. Here, layers with the same name have the same characteristics, and the description of the layer thickness of the skin layer 4 and the core surface layer 5 is the thickness after the two layers are combined.

[0071] Here, if Figure 3 As shown, the thickness of the first (upper) skin layer 4 is set to d s1 , the thickness of the second (lower) skin layer 4 is set to d s2 The thickness d of the skin layer 4 of the two layers included in the foamed molded body 10 is s is the thickness d of the first skin layer 4 s1 The thickness d of the second skin layer 4 s2 Similarly, let the thickness of the first (upper) core surface layer 5 be d f1 , the thickness of the second (lower) core surface layer 5 is set to d f2 The thickness d of the core surface layer 5 of the two layers included in the foamed molded body 10 is fis the thickness d of the first core surface layer 5 f1 The thickness d of the second core surface layer 5 f2 The total of .

[0072] <Cortex>

[0073] The skin layer 4 is a layer without foaming cells 3, and the mass concentration ratio of the amount of the fibrous filler 2 in the skin layer 4 and the amount of the fibrous filler 2 in the core inner layer 6 (the amount of fibrous filler in the skin layer / the amount of fibrous filler in the core inner layer) is preferably 1.05 or more and 1.6 or less. The ratio of the thickness of the skin layer 4 to the thickness of the entire foaming molded body 10 (skin layer thickness d s / Thickness of foamed body d a ) is preferably greater than or equal to 0.01 and less than or equal to 0.5.

[0074] If the skin layer 4 has foaming holes 3, the appearance is poor, and the elastic modulus of the surface is insufficient, and the impact resistance is reduced. When the mass concentration ratio of the amount of the fibrous filler 2 of the skin layer 4 and the core inner layer 6 is less than 1.05, the elastic modulus of the surface of the foaming molded body 10 is insufficient, and the impact resistance is reduced. When the amount ratio of the fibrous filler 2 of the skin layer 4 and the core inner layer 6 exceeds 1.6, since the interlayer strength difference of the foaming molded body 10 becomes large, the shock wave generated during the impact will not follow, and cracks are easily generated, and the impact resistance is reduced.

[0075] If the ratio of the thickness of the skin layer 4 to the thickness of the foamed molded body 10 (skin layer thickness d s / Thickness of foamed body d a ) is less than 0.01, the elastic modulus of the surface is insufficient and the impact resistance is reduced. On the other hand, if it exceeds 0.5, the overall density is affected, so that lightweighting cannot be achieved.

[0076] <Core Surface Layer>

[0077] Next, the core surface layer 5 is described. The core surface layer 5 is a layer having foamed cells 3, the mass concentration ratio of the fibrous filler 2 of the core surface layer 5 to the core inner layer 6 (fibrous filler amount of the skin layer / fibrous filler amount of the core inner layer) is 1.02 or more and 1.5 or less, and the thickness ratio of the core surface layer 5 to the thickness of the foamed molded body 10 (core surface layer thickness df / foamed molded body thickness df) is 1.02 or more and 1.5 or less. a) is greater than 0.01 and less than 0.5, and the diameter of the foamed holes 3 in the core surface layer 5 is preferably less than 80μm. The core surface layer 5 is the intermediate layer between the skin layer 4 and the core inner layer 6, which alleviates the strength difference between the skin layer 4 and the core inner layer 6 and improves the impact resistance. Therefore, it is preferred that the strength of the core surface layer 5 is the intermediate value between the strengths of the skin layer 4 and the core inner layer 6. If the diameter of the foamed holes in the core surface layer 5 exceeds 80μm, the strength difference between the part and the skin layer 4 becomes larger, and it will not follow the shock wave generated during the impact, and cracks are likely to occur, thereby reducing the impact resistance. When the mass concentration ratio of the amount of fibrous filler 2 in the core surface layer 5 and the core inner layer 6 is less than 1.02, the elastic modulus of the surface of the foamed molded body 10 is insufficient, and the impact resistance is reduced. When the mass concentration ratio of the fibrous filler 2 in the core surface layer 5 and the core inner layer 6 exceeds 1.5, the interlayer strength difference of the foamed molded body 10 becomes large, and it cannot follow the shock wave generated during the impact, and cracks are easily generated, thereby reducing the impact resistance.

[0078] If the ratio of the thickness of the core surface layer 5 to the thickness of the foamed molded body 10 (core surface layer thickness df / foamed molded body thickness df) is a ) is less than 0.01, the elastic modulus of the surface is insufficient and the impact resistance is reduced. On the other hand, if it exceeds 0.5, the overall density is affected, so that weight reduction cannot be achieved.

[0079] <Core inner layer>

[0080] Next, the core inner layer 6 in the present embodiment is described. The core inner layer 6 is a layer having foamed cells 3, and the foamed cell diameter in the core inner layer 6 is preferably 500 μm or less. If the cell diameter of the core inner layer 6 exceeds 500 μm, cracks and the like are easily formed from the portion having a larger foamed cell diameter, and the impact resistance is reduced.

[0081] <Method for producing foamed molded article>

[0082] Next, a method for producing the foamed molded article 10 will be described. Figure 4 1 is a flowchart illustrating a manufacturing process of the foaming molded body 10 of the present embodiment. (1) First, a main resin 1, a fibrous filler 2, and a dispersant as required are put into a melt-kneading treatment device and melt-kneaded in the device. Thus, the main resin 1 is melted, and the fibrous filler 2 and the dispersant are dispersed in the molten main resin 1. At the same time, the shearing action of the equipment promotes the defibration of the aggregated mass of the fibrous filler 2, and the fibrous filler 2 can be finely dispersed in the main resin 1.

[0083] Conventionally, the fibrous filler 2 is a material obtained by pre-fibrillating fibers by pre-treatment such as wet dispersion. However, when the fibrous filler 2 is pre-fibrillated in a solvent used for wet dispersion, it is easier to be fibrillated than when it is fibrillated in a molten main resin 1. Therefore, it is difficult to fibrillate only the ends, and the fibrous filler 2 may be completely fibrillated. In addition, there is a problem that the number of steps increases due to the addition of pre-treatment, and the productivity deteriorates.

[0084] In contrast, in the manufacturing process of the foamed molded body of the present embodiment, a pre-treatment based on wet dispersion for the purpose of defibration and modification of the fibrous filler 2 is not performed, but a melt-kneading process (full dry process) is performed together with the main component resin 1, the dispersant, etc. In this process, by not performing the wet dispersion process of the fibrous filler 2, only the end portion of the fibrous filler 2 can be partially defibrated as described above, and the number of steps is also small, which can improve productivity.

[0085] The composite resin composition in the present embodiment is preferably prepared by a fully dry process, and high shear stress is preferably applied during mixing. As specific mixing methods, single-axis mixers, double-axis mixers, roll mixers, Banbury mixers, etc. can be listed. From the viewpoint of being easy to apply high shear and high in mass production, continuous double-axis mixers and continuous roll mixers are particularly preferred. It should be noted that as long as it is a method that can apply high shear stress, mixing methods other than the above may also be used.

[0086] (2) The composite resin composition extruded from the melt kneading device is cut into pellets by a granulator or the like. As a method of pelletizing, there are methods that are performed immediately after the resin is melted, such as an air heat cutting method, an underwater heat cutting method, and a strand cutting method. Alternatively, there is also a pulverizing method that is performed by pulverizing or cutting after forming a primary molded body or sheet.

[0087] (3) When a chemical foaming agent is used, the pellets are dry-mixed with the chemical foaming agent before injection foam molding, and injection foam molding is performed, thereby producing an injection molded product as a foamed molded body 10. When a physical foaming agent is used, the pellets are put into an injection foam molding machine, and after melting, the physical foaming agent is injected to perform injection foam molding, thereby producing an injection molded product as a foamed molded body.

[0088] Hereinafter, each Example and each Comparative Example in the experiment performed by the present inventors will be described.

[0089] (Example 1)

[0090] A pulp-dispersed polypropylene composite foamed molded body was produced by the following production method.

[0091] As the starting material of the fibrous filler, conifer pulp (trade name: NBKP Celgar, manufactured by Mitsubishi Paper Industries, Ltd.) is used. The conifer pulp is crushed with a pulverizer to obtain a mixture of fillers with different aspect ratios of the fibrous fillers. The aspect ratios of each are adjusted by a pulverization process. Polypropylene as the main resin (trade name: J108M, manufactured by Prime Polymer Co., Ltd.), the above-mentioned fibrous filler, and maleic anhydride as a dispersant (trade name: Yumex, manufactured by Sanyo Chemical Industries, Ltd.) are weighed to a weight ratio of 42:50:5, and dry mixed. Then, melt-kneading and dispersion are performed using a twin-shaft mixer (KRC kneader manufactured by Kurimoto Iron Works Co., Ltd.). The resin melt is hot-cut to produce pulp-dispersed polypropylene pellets.

[0092] The prepared pulp-dispersed polypropylene pellets and polyslen (manufactured by Eiwa Chemical Industry Co., Ltd.) as a foaming agent were weighed to a weight ratio of 97:3 and dry-mixed. Then, a test piece of a foamed molded body was made using an injection foam molding machine (180AD manufactured by Nippon Steel Works) with a core-retracting method (Japanese: コアバック method) at a foaming ratio of 1.6 times. The production conditions of the test piece were set to a resin temperature of 190°C, a mold temperature of 40°C, an injection speed of 100mm / s, and a holding pressure of 60MPa. The respective layer structures were adjusted by the injection foaming process and the material composition. The pellets and the foaming agent were bitten into the screw of the molding machine through the hopper. The invasiveness at this time was measured by the amount of pellet reduction per hour, and it was confirmed that it was constant. The shape of the test piece was changed according to the following evaluation items, and a dumbbell of size 1 was made for measuring the elastic modulus, and a foamed molded body of 60mm square and 1.6mm thickness was made for the drop impact test and for confirming the appearance. In addition, in order to evaluate the expansion ratio, a composite resin molded body was also prepared from the above flat plate which was not foam-molded. The obtained pulp-dispersed polypropylene composite foamed molded body test piece was evaluated by the following method.

[0093] (Foaming ratio)

[0094] The expansion ratio was determined by the ratio of the apparent density of the obtained flat-plate-shaped foamed body test piece to the apparent density of the unfoamed body test piece. Here, as a method for evaluating the apparent density, the volume was calculated from the result of measuring the size of the molded body with a vernier caliper, and the apparent density was calculated from the result of measuring the weight with a precision balance, and the ratio was calculated. The result of evaluating the expansion ratio was 1.61 times.

[0095] (Bubble hole diameter)

[0096] The cross section of the obtained pulp dispersed polypropylene composite foamed body was exposed by CP treatment, and the diameter of the foamed pores was observed by SEM observation. About 10 representative foamed pores of the core surface layer and the core inner layer were measured, and the result was that the diameter of the foamed pore 3 of the core surface layer was 50 μm at most, and the diameter of the foamed pore 3 of the core inner layer was 250 μm.

[0097] (Pulp volume)

[0098] The cross section of the obtained pulp-dispersed polypropylene composite foamed molded body was exposed by CP treatment, and the infrared spectrophotometry was used to evaluate the -1 The ratio of the skin layer to the core inner layer is 1.2. The ratio of the core surface layer to the core inner layer is 1.15.

[0099] (Aspect ratio of fiber)

[0100] The obtained pulp dispersed polypropylene pellets were immersed in a xylene solvent to dissolve the polypropylene, and the fiber shape of the remaining pulp fibers was observed by SEM. About 50 representative fibers were measured at 5 locations, and the results showed that the ratio of the aspect ratio being 10 or more was 5-10%, and the ratio of the aspect ratio being 2 or less was 50-60%.

[0101] (Elastic modulus of foamed article)

[0102] The obtained dumbbell-shaped test piece No. 1 was used to perform a tensile test. Here, as a method for evaluating the elastic modulus, a value less than 1.6 GPa was set as ×, a value greater than 1.6 GPa and less than 2.0 GPa was set as ○, and a value greater than 2.0 GPa was set as ◎. The elastic modulus of the test piece was 2.5 GPa, and its evaluation was ◎.

[0103] (Results of drop test of foamed article)

[0104] The obtained flat plate-shaped test piece was subjected to a drop impact test. Specifically, a heavy cone weighing 250 g was dropped from a height of 80 cm onto the plate surface of the test piece to check whether there were cracks. As an evaluation method, a sample with no cracks was marked as ○, a sample with cracks only on the surface and the length of the cracks less than 10 mm was marked as △, and a sample with through cracks or cracks with a length of more than 10 mm was marked as ×. The sample with no cracks was evaluated as ○.

[0105] (Lightweight ratio)

[0106] The specific stiffness (Japanese: 比剛性) is calculated from the results of the apparent density and the elastic modulus during the above-mentioned calculation of the foaming ratio, and the weight reduction rate is calculated from the ratio of the specific stiffness to that of the polypropylene monomer. Here, as an evaluation method for the weight reduction rate, a value less than 15% is set as ×, a value of 15% or more and less than 20% is set as ○, and a value of 20% or more is set as ◎. The result of calculating the weight reduction rate is 32%, which is ◎.

[0107] (Appearance of the foamed molded body)

[0108] A sensory evaluation is performed on whether aggregates of fibers horizontal to the eye can be seen as white spots and whether traces of air bubbles can be seen on the foamed molded body. A foamed molded body without white spots and air bubble traces is set as ○, and the presence of white spots and air bubble traces is set as △.

[0109] (Example 2)

[0110] In Example 2, polypropylene, cotton-like softwood pulp, and maleic anhydride were weighed so that the weight ratio was 62:30:5, and dry mixing was performed. The target foaming ratio was changed to 1.8 times, and the other material conditions and process conditions were the same as those in Example 1, to produce pulp-dispersed polypropylene pellets and a foamed molded body. Regarding the evaluation, the same evaluation as in Example 1 was also performed.

[0111] (Example 3)

[0112] In Example 3, polypropylene, cotton-like softwood pulp, and maleic anhydride were weighed so that the weight ratio was 22:70:5, and dry mixing was performed. The target foaming ratio was changed to 1.3 times, and pulp-dispersed polypropylene pellets and polyslen were weighed so that the weight ratio was 99:1. The other material conditions and process conditions were the same as those in Example 1, to produce pulp-dispersed polypropylene pellets and a foamed molded body. Regarding the evaluation, the same evaluation as in Example 1 was also performed.

[0113] (Example 4)

[0114] In Example 4, the pulverization time of the pulp was lengthened, and the other material conditions and process conditions were the same as those in Example 1, to produce pulp-dispersed polypropylene pellets and a foamed molded body. Regarding the evaluation, the same evaluation as in Example 1 was also performed.

[0115] (Example 5)

[0116] In Example 5, the pulverization time of the pulp was shortened, and the other material conditions and process conditions were the same as those in Example 1, to produce pulp-dispersed polypropylene pellets and a foamed molded body. Regarding the evaluation, the same evaluation as in Example 1 was also performed.

[0117] (Comparative Example 1)

[0118] In Comparative Example 1, polypropylene, cotton-like conifer pulp and maleic anhydride were weighed to a weight ratio of 82:10:5, and dry-mixed, and the target expansion ratio was changed to 1.6 times. Other material conditions and process conditions were the same as those in Example 1 to produce pulp-dispersed polypropylene pellets and foamed molded products. The same evaluation as in Example 1 was also performed for evaluation.

[0119] (Comparative Example 2)

[0120] In Comparative Example 2, polypropylene, cotton-like conifer pulp and maleic anhydride were weighed to a weight ratio of 22:70:5, and dry-mixed, and the target foaming ratio was changed to 1.05 times, and pulp-dispersed polypropylene pellets and polyslen were weighed to a weight ratio of 99.995:0.005. Other material conditions and process conditions were the same as those in Example 1, and pulp-dispersed polypropylene pellets and foamed molded products were prepared. The same evaluation as in Example 1 was also performed for evaluation.

[0121] (Comparative Example 3)

[0122] In Comparative Example 3, polypropylene, cotton-like conifer pulp, and maleic anhydride were weighed to a weight ratio of 22:70:5, and dry-mixed, and the target expansion ratio was changed to 1.05 times. Other material conditions and process conditions were the same as those in Example 1 to produce pulp-dispersed polypropylene pellets and foamed molded products. The same evaluation as in Example 1 was also performed for evaluation.

[0123] The measurement results of Examples 1 to 5 and Comparative Examples 1 to 3 are shown in FIG. Figure 5 .

[0124] from Figure 5 It can be seen that the result of Example 2, in which the content of fibrous filler is reduced and the foaming ratio is increased, is that the elastic modulus is slightly poor, but the reduction in impact resistance can be suppressed by the effects of the skin layer and the core surface layer. On the contrary, the result of Example 3, in which the amount of fibrous filler is increased and the foaming ratio is reduced, is that the lightweight is slightly poor, but the fibrous fillers of different aspect ratios are mixed, and there are no foaming holes in the skin layer, so the deterioration of the appearance can be suppressed. The elastic modulus of Example 4, in which the amount of fibrous filler with an aspect ratio of 10 is reduced, is slightly reduced, but it can be confirmed that there is no problem. It can be confirmed that if it contains 10 to 85% by mass of the main resin, 15 to 85% by mass of the filler, 0.01 to 20% by mass of the dispersant, 0.01 to 15% by mass of the foaming agent, and the foaming ratio is 1.1 times or more, a foamed molded body that takes into account both high strength and lightweight can be obtained.

[0125] In Comparative Example 1, in which the amount of fibrous filler was reduced to 10%, the amount of fibrous filler was small, and therefore the elastic modulus was insufficient. In addition, since the fibrous filler also acted as a foaming nucleus, the diameter of the foaming cells 3 also became larger. As a result, the impact resistance was reduced, and cracks were generated in the impact test.

[0126] In the embodiment 5 that increases the fiber-like filler aspect ratio and is the ratio of the fiber more than 10, the result is that, although the elastic modulus increases a little, the impact resistance decreases, and cracks are generated in the impact test. In addition, due to the large fiber of aspect ratio, white spots can be observed in the foaming molding.

[0127] In Comparative Example 2, in which the amount of the blowing agent was reduced to 0.005%, the expansion ratio was lower than the target expansion ratio. In addition, since the amount of the blowing agent as the foaming core was very small, the foam cell diameter became larger, and although there was no problem with the elastic modulus, it became uneven, the impact resistance decreased, and cracks occurred in the impact test.

[0128] In Comparative Example 3 in which the expansion ratio was reduced to 1.05, it was found that although there were no problems with the elastic modulus and impact resistance due to the small expansion ratio, the weight reduction could not be achieved.

[0129] According to the above evaluation, the composite resin composition in the foaming molded body contains 10% by mass or more and 85% by mass or less of the main resin, 15% by mass or more and 85% by mass or less of the filler, and 0.01% by mass or less and 15% by mass or less of the foaming agent, and the foaming ratio brought by the foaming agent is more than 1.1 times, thereby achieving high strength and lightness. It is further known that when the fiber presence ratio of the added fibrous filler is more than 10 and the fiber presence ratio of the fiber with an aspect ratio of less than 2 is more than 50% and less than 70%, a foaming molded body with no fiber agglomerates and good appearance can be obtained.

[0130] It should be noted that the present invention includes embodiments and / or examples obtained by appropriately combining any of the various embodiments and / or examples described above, and can achieve the effects possessed by each embodiment and / or example.

[0131] As described above, according to the foamed molded article of the present invention, it is possible to achieve both high impact resistance and light weight and excellent appearance.

[0132] Industrial Applicability

[0133] According to the foaming molding of the present invention, a foaming molding having excellent mechanical strength than conventional general-purpose resins can be provided. According to the present invention, since the characteristics of the main agent resin can be improved, it can be used as a substitute for engineering plastics or a substitute for metal materials. Therefore, the manufacturing cost of various industrial products or daily necessities made of engineering plastics or metals can be greatly reduced. And then it can be used for household appliance housings, building materials, and automobile components.

Claims

1. A foamed molded body, comprising: Thermoplastic resin as main resin; A mixture of cellulose-based fibrous fillers having different aspect ratios; and The foaming holes formed by the foaming agent, The foaming ratio of the foaming agent is 1.1 times or more.

2. The foamed molded article according to claim 1, The foamed molded body has The surface cortex, A core surface layer located inside the skin layer and having a mass concentration of the filler lower than that of the skin layer, and A core inner layer is located inside the core surface layer and has a lower mass concentration of the filler than the core surface layer.

3. The foamed molded article according to claim 2, The ratio of the mass concentration of the filler in the skin layer to the mass concentration of the filler in the core inner layer is 1.05 or more, and the ratio of the mass concentration of the filler in the core surface layer to the mass concentration of the filler in the core inner layer is 1.02 or more.

4. The foamed molded article according to claim 2 or 3, The cell diameter of the foaming agent contained in the core surface layer is smaller than the cell diameter of the foaming agent contained in the core inner layer.

5. The foamed molded article according to claim 4, The cell diameter of the foaming agent contained in the core surface layer is 40 μm to 80 μm, and the cell diameter of the foaming agent contained in the core inner layer is 90 μm to 500 μm.

6. The foamed molded body according to any one of claims 1 to 5, The filler includes a filler having an aspect ratio of 2 or less and a filler having an aspect ratio of 10 or more.

7. The foamed molded article according to claim 6, The proportion of the filler having an aspect ratio of 2 or less is greater than the proportion of the filler having an aspect ratio of 10 or more.

8. The foamed molded article according to claim 7, The proportion of fillers having an aspect ratio of 2 or less among the fillers is 50% to 70% inclusive, and the proportion of fillers having an aspect ratio of 10 or more among the fillers is 1% to 10% inclusive.