High-thermal-conductivity infrared disguise hillstone-like thin shell as well as preparation method and application thereof
By using composite layer structure of epoxy resin, thermal filler and glass fiber layer in the imitation rock shell of the camouflage door, the problem of low thermal conductivity of existing materials is solved, and high thermal conductivity and low infrared exposure risks are achieved, satisfying the Infrared radiation temperature difference requirements for camouflage design specifications in national defense engineering.
Patent Information
- Application Number
- CN202411032194.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-19
AI Technical Summary
The existing camouflage doors have low thermal conductivity, which makes the heat generated by solar radiation unable to be quickly transferred, increasing the risk of infrared exposure.
Using a composite layer structure composed of epoxy resin, thermal filler, accelerator, initiator and glass fiber layer, a high-thermal conductivity infrared camouflage imitation stone thin shell is prepared through layered structure and coating molding process, and using hexagonal phase nitriding Boron is used as a thermal filler to build an efficient thermal filler network.
It significantly improves the thermal conductivity of the material, reduces the risk of infrared exposure, and meets the infrared radiation temperature difference requirements of the "GJB4149-2000 National Defense Engineering Camouflage Design Specification".
Smart Images

Figure CN118978789A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of camouflage materials, and in particular relates to a preparation method and application of a high thermal conductivity infrared camouflage imitation rock thin shell. Background Art
[0002] For projects that need to be hidden inside a mountain, the entrance of the project is usually disguised as the topographical features of the surrounding mountain, so as to achieve the purpose of effectively hiding the truth and showing the false. Therefore, the entrance of the project is the key part of the camouflage. At the entrance of the project, a thin shell imitating a mountain stone is often used to make a camouflaged door.
[0003] However, the imitation stone thin shells commonly used in existing camouflage doors are mostly made of cement direct plastic technology and polymer materials. The thermal conductivity of such materials is almost all concentrated in the range of 0.1-0.5W / mk. Therefore, it is impossible to quickly and efficiently transfer the heat generated by solar radiation to the phase change material, causing the heat to accumulate in the imitation stone thin shell on the surface, greatly increasing the risk of infrared exposure of the camouflage door.
[0004] In view of this, this invention is proposed. Summary of the invention
[0005] In view of the shortcomings of the prior art, the present invention proposes a high thermal conductivity infrared camouflage imitation rock thin shell, which has good thermal conductivity and can prevent target infrared exposure.
[0006] To achieve the above object, the present invention adopts the following technical solutions:
[0007] The present invention provides a high thermal conductivity infrared camouflage imitation rock thin shell, which is a layered structure consisting of a composite layer and a glass fiber layer. The composite layer consists of epoxy resin, accelerator, initiator, talcum powder and thermal conductive filler.
[0008] Preferably, the composite layer is composed of the following parts by weight: 10 to 40 parts of epoxy resin, 0.5 to 2 parts of accelerator, 0.5 to 2 parts of initiator, 5 to 10 parts of talc, and 50 to 80 parts of thermal conductive filler.
[0009] Preferably, the glass fiber layer is composed of 7628 glass fiber cloth.
[0010] Preferably, the epoxy resin is 6101 type epoxy resin, the accelerator is cobalt isooctanoate accelerator, and the initiator is methyl ethyl ketone peroxide.
[0011] Preferably, the thermally conductive filler is hexagonal boron nitride.
[0012] Preferably, the imitation rock thin shell has 5 layers, from bottom to top, the first, third and fifth layers are composite layers, and the second and fourth layers are glass fiber layers.
[0013] Preferably, the thickness of the composite layer and the glass fiber layer are both 2 mm.
[0014] The present invention also provides a method for preparing a high thermal conductivity infrared camouflage imitation rock thin shell, comprising the following steps:
[0015] S1, pouring the epoxy resin and the thermal conductive filler into a mixing container and stirring for the first time until the mixture is uniform, to obtain a mixture a;
[0016] S2, adding a accelerator, an initiator, and talcum powder to the mixture a, and stirring for a second time until the mixture is uniform, to obtain a mixture b;
[0017] S3, applying a composite layer and a glass fiber layer on the bottom surface of a rectangular mold in the shape of a rock surface, wherein the composite layer is formed by applying mixture b;
[0018] S4. The mold is transferred to an oven, and after drying, the mold is demoulded to obtain a high thermal conductivity infrared camouflage imitation rock thin shell.
[0019] Preferably, the stirring speed of the first stirring in S1 is 500-800 r / min, and the stirring time is 10-15 min; the stirring speed of the second stirring in S2 is 200-500 r / min, and the stirring time is 5-10 min; the drying temperature in S4 is 60° C., and the drying time is 6 h.
[0020] The present invention also proposes the use of a high thermal conductivity infrared camouflage imitation rock thin shell in the preparation of a camouflaged door.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] The high thermal conductivity infrared camouflage imitation rock thin shell provided by the present invention is composed of a composite layer and a glass fiber cloth. Compared with the traditional anti-rock thin shell, the composite layer of the present invention uses boron nitride with a thermal conductivity of 56.94w / (mk) as a thermal conductive filling filler, which solves the problem of target infrared exposure caused by low thermal conductivity of epoxy resin-based imitation rock thin shell. With the high thermal conductivity of boron nitride as the goal and the construction of an efficient thermal conductive filler network as the key idea, a coating molding process is adopted to prepare a high thermal conductivity infrared camouflage imitation rock thin shell. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] The accompanying drawings are incorporated in and constitute a part of this specification and, together with the description, serve to explain the principles of the present invention.
[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0025] Figure 1 A schematic diagram of the structure of the imitation rock thin shell prepared by the present invention applied to a camouflaged door;
[0026] Figure 2 Infrared radiation images of the imitation mountain stone thin shell prepared in an embodiment of the present invention and a common imitation mountain stone thin shell after being installed on the surface of a camouflaged door.
[0027] Figure numerals: 1. Engineering steel frame structure, 2. Heat insulation layer, 3. Radar absorbing layer, 4. Phase change layer, 5. High thermal conductivity infrared camouflage imitation rock thin shell, 6. High thermal conductivity infrared camouflage imitation rock thin shell area, 7. Ordinary imitation rock thin shell area, 8. Background wall. DETAILED DESCRIPTION
[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Example 1
[0030] A high thermal conductivity infrared camouflage imitation rock thin shell has a layered structure with five layers. From bottom to top, the first, third and fifth layers are composite layers, and the second and fourth layers are glass fiber layers. The composite layer is composed of the following components by mass: 10 parts of 6101 epoxy resin, 0.5 parts of cobalt isooctanoate, 0.5 parts of methyl ethyl ketone peroxide, 9 parts of talcum powder, and 80 parts of hexagonal boron nitride; the glass fiber layer is made of 7628 glass fiber cloth.
[0031] The method for preparing the high thermal conductivity infrared camouflage imitation rock thin shell comprises the following steps:
[0032] S1. Pour 6101 epoxy resin and hexagonal boron nitride into a mixing container and stir evenly at a stirring speed of 500 r / min for 15 min, so that there are no obvious bubbles and unmixed particles in the mixture, to obtain a mixture a;
[0033] S2, add cobalt isooctanoate, methyl ethyl ketone peroxide and talcum powder to mixture a and stir again, the stirring speed is 200r / min, the stirring time is 10min, so that there are no obvious bubbles and unmixed particles in the mixture, to obtain mixture b;
[0034] S3. Pour mixture b into a rectangular mold with a rock-like surface shape. After the mixture completely covers the bottom of the mold, use a KTQ-II type coating device to control the coating thickness to 2 mm. After scraping off the excess slurry, form the first composite layer. Cover the surface of the first layer with 7628 glass fiber cloth with a thickness of 2 mm to form the second glass fiber layer. Use a scraper to scrape off the bubbles between the second layer and the first layer to make the two fit completely. Pour mixture b onto the surface of the second glass fiber layer. After the mixture completely covers the surface of the second layer, use K The coating thickness is controlled to be 2mm by the TQ-II type coating device, and the third composite layer is formed after scraping off the excess slurry; the surface of the third composite layer is covered with 7628 glass fiber cloth with a thickness of 2mm to form the fourth glass fiber layer, and the air bubbles between the third and fourth layers are scraped off with a scraper to make the two layers fit completely; the mixture b is poured onto the surface of the fourth glass fiber layer, and after the mixture completely covers the surface of the fourth layer, the coating thickness is controlled to be 2mm by the KTQ-II type coating device, and the fifth composite layer is formed after scraping off the excess slurry;
[0035] S4. Transfer the mold to an oven and bake at 60°C for 6 hours. Take it out and demould it to obtain a high thermal conductivity infrared camouflage imitation rock thin shell.
[0036] After the high thermal conductivity infrared camouflage imitation rock thin shell is installed on the surface of the camouflaged door, the infrared radiation temperature difference between it and the background is shown in Table 1.
[0037] Example 2
[0038] A high thermal conductivity infrared camouflage imitation rock thin shell has a layered structure with five layers. From bottom to top, the first, third and fifth layers are composite layers, and the second and fourth layers are glass fiber layers. The composite layer is composed of the following components by mass: 20 parts of 6101 epoxy resin, 1.5 parts of cobalt isooctanoate, 1.5 parts of methyl ethyl ketone peroxide, 7 parts of talcum powder, and 70 parts of hexagonal boron nitride; the glass fiber layer is made of 7628 glass fiber cloth.
[0039] The method for preparing the high thermal conductivity infrared camouflage imitation rock thin shell comprises the following steps:
[0040] S1. Pour 6101 epoxy resin and hexagonal boron nitride into a mixing container and stir evenly at a stirring speed of 600 r / min for 12 min, so that there are no obvious bubbles and unmixed particles in the mixture, to obtain a mixture a;
[0041] S2, add cobalt isooctanoate, methyl ethyl ketone peroxide and talcum powder to the mixture a and stir again, the stirring speed is 300r / min, the stirring time is 7min, so that there are no obvious bubbles and unmixed particles in the mixture, to obtain a mixture b;
[0042] S3. Pour mixture b into a rectangular mold with a rock-like surface shape. After the mixture completely covers the bottom of the mold, use a KTQ-II type coating device to control the coating thickness to 2 mm. After scraping off the excess slurry, form the first composite layer. Cover the surface of the first layer with 7628 glass fiber cloth with a thickness of 2 mm to form the second glass fiber layer. Use a scraper to scrape off the bubbles between the second layer and the first layer to make the two fit completely. Pour mixture b onto the surface of the second glass fiber layer. After the mixture completely covers the surface of the second layer, use K The coating thickness is controlled to be 2mm by the TQ-II type coating device, and the third composite layer is formed after scraping off the excess slurry; the surface of the third composite layer is covered with 7628 glass fiber cloth with a thickness of 2mm to form the fourth glass fiber layer, and the air bubbles between the third and fourth layers are scraped off with a scraper to make the two layers fit completely; the mixture b is poured onto the surface of the fourth glass fiber layer, and after the mixture completely covers the surface of the fourth layer, the coating thickness is controlled to be 2mm by the KTQ-II type coating device, and the fifth composite layer is formed after scraping off the excess slurry;
[0043] S4. Transfer the mold to an oven and bake at 60°C for 6 hours. Take it out and demould it to obtain a high thermal conductivity infrared camouflage imitation rock thin shell.
[0044] After the high thermal conductivity infrared camouflage imitation rock thin shell is installed on the surface of the camouflaged door, the infrared radiation temperature difference between it and the background is shown in Table 1.
[0045] Example 3
[0046] A high thermal conductivity infrared camouflage imitation rock thin shell has a layered structure with five layers. From bottom to top, the first, third and fifth layers are composite layers, and the second and fourth layers are glass fiber layers. The composite layers are composed of the following components by mass: 40 parts of 6101 epoxy resin, 1 part of cobalt isooctanoate, 1 part of methyl ethyl ketone peroxide, 8 parts of talcum powder, and 50 parts of hexagonal boron nitride; the glass fiber layer is made of 7628 glass fiber cloth.
[0047] The method for preparing the high thermal conductivity infrared camouflage imitation rock thin shell comprises the following steps:
[0048] S1. Pour 6101 epoxy resin and hexagonal boron nitride into a mixing container and stir evenly at a stirring speed of 800 r / min for 10 min, so that there are no obvious bubbles and unmixed particles in the mixture, to obtain a mixture a;
[0049] S2, add cobalt isooctanoate, methyl ethyl ketone peroxide and talcum powder to mixture a and stir again, the stirring speed is 500r / min, the stirring time is 5min, so that there are no obvious bubbles and unmixed particles in the mixture, to obtain mixture b;
[0050] S3. Pour mixture b into a rectangular mold with a rock-like surface shape. After the mixture completely covers the bottom of the mold, use a KTQ-II type coating device to control the coating thickness to 2 mm. After scraping off the excess slurry, form the first composite layer. Cover the surface of the first layer with 7628 glass fiber cloth with a thickness of 2 mm to form the second glass fiber layer. Use a scraper to scrape off the bubbles between the second layer and the first layer to make the two fit completely. Pour mixture b onto the surface of the second glass fiber layer. After the mixture completely covers the surface of the second layer, use K The coating thickness is controlled to be 2mm by the TQ-II type coating device, and the third composite layer is formed after scraping off the excess slurry; the surface of the third composite layer is covered with 7628 glass fiber cloth with a thickness of 2mm to form the fourth glass fiber layer, and the air bubbles between the third and fourth layers are scraped off with a scraper to make the two layers fit completely; the mixture b is poured onto the surface of the fourth glass fiber layer, and after the mixture completely covers the surface of the fourth layer, the coating thickness is controlled to be 2mm by the KTQ-II type coating device, and the fifth composite layer is formed after scraping off the excess slurry;
[0051] S4. Transfer the mold to an oven and bake at 60°C for 6 hours. Take it out and demould it to obtain a high thermal conductivity infrared camouflage imitation rock thin shell.
[0052] After the high thermal conductivity infrared camouflage imitation rock thin shell is installed on the surface of the camouflaged door, the infrared radiation temperature difference between it and the background is shown in Table 1.
[0053] Example 4
[0054] A high thermal conductivity infrared camouflage imitation rock thin shell has a layered structure with five layers. From bottom to top, the first, third and fifth layers are composite layers, and the second and fourth layers are glass fiber layers. The composite layer is composed of the following components by mass: 33 parts of 6101 epoxy resin, 1.2 parts of cobalt isooctanoate, 1.8 parts of methyl ethyl ketone peroxide, 6 parts of talcum powder, and 58 parts of hexagonal boron nitride; the glass fiber layer is made of 7628 glass fiber cloth.
[0055] The method for preparing the high thermal conductivity infrared camouflage imitation rock thin shell comprises the following steps:
[0056] S1. Pour 6101 epoxy resin and hexagonal boron nitride into a mixing container and stir evenly at a stirring speed of 700 r / min for 13 min until there are no obvious bubbles and unmixed particles in the mixture, to obtain a mixture a;
[0057] S2, add cobalt isooctanoate, methyl ethyl ketone peroxide and talcum powder to the mixture a and stir again, the stirring speed is 400r / min, the stirring time is 8min, so that there are no obvious bubbles and unmixed particles in the mixture, to obtain a mixture b;
[0058] S3. Pour mixture b into a rectangular mold with a rock-like surface shape. After the mixture completely covers the bottom of the mold, use a KTQ-II type coating device to control the coating thickness to 2 mm. After scraping off the excess slurry, form the first composite layer. Cover the surface of the first layer with 7628 glass fiber cloth with a thickness of 2 mm to form the second glass fiber layer. Use a scraper to scrape off the bubbles between the second layer and the first layer to make the two fit completely. Pour mixture b onto the surface of the second glass fiber layer. After the mixture completely covers the surface of the second layer, use K The coating thickness is controlled to be 2mm by the TQ-II type coating device, and the third composite layer is formed after scraping off the excess slurry; the surface of the third composite layer is covered with 7628 glass fiber cloth with a thickness of 2mm to form the fourth glass fiber layer, and the air bubbles between the third and fourth layers are scraped off with a scraper to make the two layers fit completely; the mixture b is poured onto the surface of the fourth glass fiber layer, and after the mixture completely covers the surface of the fourth layer, the coating thickness is controlled to be 2mm by the KTQ-II type coating device, and the fifth composite layer is formed after scraping off the excess slurry;
[0059] S4. Transfer the mold to an oven and bake at 60°C for 6 hours. Take it out and demould it to obtain a high thermal conductivity infrared camouflage imitation rock thin shell.
[0060] After the high thermal conductivity infrared camouflage imitation rock thin shell is installed on the surface of the camouflaged door, the infrared radiation temperature difference between it and the background is shown in Table 1.
[0061] In the above embodiments, the 6101 epoxy resin, with its good fluidity and plasticity, can better adapt to the rectangular molds of various shapes and sizes of imitation stone surface shapes used in the production of high thermal conductivity infrared camouflage imitation stone thin shells. At the same time, its good strength, hardness, and corrosion resistance can enhance the weather resistance of the high thermal conductivity infrared camouflage imitation stone thin shells.
[0062] Cobalt 2-ethylhexanoate accelerator, provided by Shanghai Fudao Chemical Technology Co., Ltd., is a highly efficient unsaturated resin accelerator. Cobalt 2-ethylhexanoate accelerator can effectively promote the curing reaction of epoxy resin, improve the curing effect and the mechanical properties of the finished product.
[0063] Methyl ethyl ketone peroxide, provided by Shangshan Dongjinghai New Materials Co., Ltd. Methyl ethyl ketone peroxide can effectively initiate the polymerization reaction of the resin, providing a stable curing speed and good curing performance.
[0064] Example 5
[0065] refer to Figure 1The camouflaged door includes an engineering steel frame structure 1, a heat insulation layer 2 is arranged on the upper surface of the engineering steel frame structure 1, a radar absorbing layer 3 is arranged on the upper surface of the heat insulation layer 2, a phase change layer 4 is arranged on the upper surface of the radar absorbing layer 3, and a high thermal conductivity infrared camouflage imitation rock thin shell 5 is arranged on the upper surface of the phase change layer 4.
[0066] refer to Figure 2 After the high thermal conductivity infrared camouflage imitation mountain stone thin shell and the ordinary imitation mountain stone thin shell prepared in Examples 1 to 4 are covered on the surface of the camouflaged door, the infrared radiation temperature difference between the high thermal conductivity infrared camouflage imitation mountain stone thin shell area 6 and the ordinary imitation mountain stone thin shell area 7 and the background wall 8 is shown in Table 1.
[0067] Table 1 Infrared radiation temperature record table
[0068]
[0069] The high thermal conductivity infrared camouflage imitation rock thin shell provided by the present invention, after being installed on the surface of the camouflaged door, has an infrared radiation temperature difference with the background at all times of the day that is less than 4°C, meeting the index requirements of "GJB4149-2000 National Defense Engineering Camouflage Design Specification".
[0070] The present invention can also be composed of other numbers of layers. From bottom to top, the composite layers and the glass fiber layers are arranged alternately, and the bottom layer and the top layer are both composite layers. For example, the high thermal conductivity infrared camouflage imitation rock thin shell is a layered structure with three layers. From bottom to top, the first and third layers are composite layers, and the second layer is a glass fiber layer; or the high thermal conductivity infrared camouflage imitation rock thin shell is a layered structure with seven layers. From bottom to top, the first, third, fifth and seventh layers are composite layers, and the second, fourth and sixth layers are glass fiber layers. The thickness of each layer can be determined according to design requirements.
[0071] The specific embodiments of the present invention enable those skilled in the art to understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention.
[0072] It should be understood that the present invention is not limited to what has been described above and that various modifications and changes may be made without departing from its scope. The scope of the present invention is limited only by the appended claims.
Claims
1. A high thermal conductivity infrared camouflage imitation rock thin shell, characterized in that: The imitation rock thin shell is a layered structure, consisting of a composite layer and a glass fiber layer, wherein the composite layer consists of epoxy resin, accelerator, initiator, talcum powder and thermal conductive filler.
2. The high thermal conductivity infrared camouflage imitation rock thin shell according to claim 1, characterized in that: The composite layer is composed of the following parts by weight: 10 to 40 parts of epoxy resin, 0.5 to 2 parts of accelerator, 0.5 to 2 parts of initiator, 5 to 10 parts of talc powder, and 50 to 80 parts of thermal conductive filler.
3. The high thermal conductivity infrared camouflage imitation rock thin shell according to claim 1, characterized in that: The glass fiber layer is composed of 7628 glass fiber cloth.
4. The high thermal conductivity infrared camouflage imitation rock thin shell according to claim 1, characterized in that: The epoxy resin is 6101 type epoxy resin, the accelerator is cobalt isooctanoate accelerator, and the initiator is methyl ethyl ketone peroxide.
5. The high thermal conductivity infrared camouflage imitation rock thin shell according to claim 1, characterized in that: The thermal conductive filler is hexagonal boron nitride.
6. The high thermal conductivity infrared camouflage imitation rock thin shell according to claim 1, characterized in that: The imitation rock thin shell has 5 layers, from bottom to top, the first, third and fifth layers are composite layers, and the second and fourth layers are glass fiber layers.
7. The high thermal conductivity infrared camouflage imitation rock thin shell according to claim 1, characterized in that: The thickness of the composite layer and the glass fiber layer are both 2 mm.
8. A method for preparing a high thermal conductivity infrared camouflage imitation rock thin shell according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1, pouring the epoxy resin and the thermal conductive filler into a mixing container and stirring for the first time until the mixture is uniform, to obtain a mixture a; S2, adding a accelerator, an initiator, and talcum powder to the mixture a, and stirring for a second time until the mixture is uniform, to obtain a mixture b; S3. Apply a composite layer and a glass fiber layer on the bottom surface of a rectangular mold shaped like a rock surface, wherein the composite layer is formed by applying mixture b. S4. The mold is transferred to an oven, and after drying, the mold is demoulded to obtain a high thermal conductivity infrared camouflage imitation rock thin shell.
9. The method for preparing a high thermal conductivity infrared camouflage imitation rock thin shell according to claim 8, characterized in that: The stirring speed of the first stirring in S1 is 500-800 r / min, and the stirring time is 10-15 min; the stirring speed of the second stirring in S2 is 200-500 r / min, and the stirring time is 5-10 min; the drying temperature in S4 is 60° C., and the drying time is 6 h.
10. Use of the high thermal conductivity infrared camouflage imitation rock thin shell as claimed in any one of claims 1 to 7 in the preparation of camouflaged doors.