Water-based two-component intermediate coating and application thereof

Through the use of water-based two-component paint, the synergistic effect of aqueous hydroxyacrylate and aqueous polyurethane dispersion is used to solve the construction difficulties of water-based paint in high temperature, low temperature or high humidity environments, and achieve no need for grinding High adhesion and excellent gloss improve construction efficiency and safety.

CN118978840APending Publication Date: 2024-11-19北京钰林化工有限公司
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411134014.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing water-based medium paint has problems such as spray sag, fly ash, and difficulty in receiving guns when constructing in high-temperature, low-temperature or high-humidity environments, and requires polishing to ensure interlayer adhesion, which reduces construction efficiency and increases costs.

Method used

Provided is an aqueous two-component painted paint consisting of components A and components B, which include aqueous hydroxyacrylate dispersions, aqueous polycarbonate aliphatic anionic polyurethane dispersions and low glass transition temperatures. The aqueous aliphatic anionic polyurethane dispersion forms excellent leveling, rock-striking resistance and chemical resistance through specific proportions and synergistic effects. The paint film has a gloss of 60-80 and is not required to be polished and The topcoat adheres well.

Benefits of technology

Large-area construction is achieved under high temperature, low temperature or high humidity environments, the paint film joints are smooth, the spraying does not sag or fly ash, and the interlayer adhesion is excellent, which reduces the construction cost and accident risk of rail transit vehicles and increases the Construction efficiency and inspection accuracy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004998819890000091
    Figure BDA0004998819890000091
  • Figure BDA0004998819890000161
    Figure BDA0004998819890000161
  • Figure BDA0004998819890000171
    Figure BDA0004998819890000171
Patent Text Reader

Abstract

The invention relates to the technical field of coatings for vehicles, and particularly discloses a water-based two-component intermediate coating and application thereof. The water-based two-component intermediate paint selects a water-based hydroxyl-containing acrylate dispersion and a water-based polycarbonate-containing aliphatic anion polyurethane dispersion with high glass transition temperature to be compounded as film-forming resin, and a water-based aliphatic anion polyurethane dispersion with low glass transition temperature is selectively added to the water-based hydroxyl-containing acrylate dispersion and the water-based polycarbonate-containing aliphatic anion polyurethane dispersion. Through a specific ratio and a synergistic effect of the components, the characteristics of different types of water-based resins are brought into play to an optimal state, so that the water-based two-component intermediate coating has excellent leveling property, thixotropy, elasticity and interlayer adhesive force, does not fly ash, has excellent mechanical properties and weather resistance, and can be widely applied to the field of water-based coating. According to the present invention, large-area construction can be performed in the high-temperature, low-temperature or high-humidity environment, especially the intermediate coat does not need to be polished before and after coating, the interlayer adhesion with the primer and the finishing coat is excellent, the appearance gloss is excellent, and the high practical value and the high promotion value are provided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of automotive coatings, and in particular to a water-based two-component mid-coat and application thereof. Background Art

[0002] Rail transit vehicles are a major means of transportation for the public. Rail transit vehicles are mostly manufactured using lightweight aluminum alloys instead of steel. With the change in the material of the carriages, the types and quality of coatings have also changed. Rail transit vehicles operate in various environments from C2 to C5, which determines that their coatings must take into account both anti-corrosion and decorative effects. The traditional rail transit vehicle body surface coating system is a solvent-based paint, and VOC (volatile organic compound) emissions account for more than 60% of the total coating volume, which not only wastes resources, but also pollutes the environment, and also poses a fire hazard. The water-based paint coating system has a low VOC content, is green and environmentally friendly, is safe and convenient to construct, and has a good paint film appearance and excellent overall performance. It has become the mainstream direction of the development of the modern coatings industry.

[0003] At present, the surface coating of rail transit vehicle bodies is a multi-layer system, usually including a primer layer, a mid-coat layer and a topcoat layer, among which the mid-coat is between the primer, putty and topcoat. As an intermediate paint that connects the upper and lower paint layers, its main function is to further fill and correct the surface of the workpiece that has been primed, improve the flatness, so as to improve the vividness, fullness and gloss of the topcoat, and improve the stone impact resistance of the coating. However, the water-based mid-coat used in rail transit vehicles has high requirements for the construction environment. Due to the large construction area of ​​the rail transit vehicle body painting, there are spray sags, fly ash, and difficulty in connecting the gun when the mid-coat is applied in an environment with high temperature, low temperature or high humidity; and in order to ensure the interlayer adhesion of the coating, the primer coating needs to be polished before the mid-coat is applied. After the mid-coat is applied and dried, the mid-coat needs to be polished before the topcoat is applied. The polishing process reduces the construction efficiency and increases the construction cost. Therefore, the existing water-based mid-coat must be applied under constant temperature and humidity conditions. In order to solve the problems of low gloss and harsh construction conditions of existing water-based mid-coat paints, it is urgent to find a water-based mid-coat paint that can be constructed in high temperature, low temperature or high humidity environments, with a smooth transition at the paint film joint, a flat and smooth surface, no fly ash when spraying over a large area, and excellent interlayer adhesion between the previous primer layer and the next topcoat layer without polishing, so as to meet the actual needs of the application of water-based mid-coat paint in rail transit vehicle painting. Summary of the invention

[0004] In view of the above problems, the present invention provides a water-based two-component mid-coat and its application. The water-based two-component mid-coat has excellent thixotropy, adhesion, filling, polishing, physical and mechanical and chemical properties, can be constructed on a large area under high temperature, low temperature or high humidity environments, and the paint film joint has a smooth transition, and there is no sag or fly ash during spraying; the paint film is flat and smooth, and the interlayer adhesion between the mid-coat and the primer and topcoat is excellent. In particular, the mid-coat does not need to be polished before and after painting, and the interlayer adhesion can reach level 0.

[0005] In order to solve the above technical problems, the technical solution provided by the present invention is:

[0006] In a first aspect, the present invention provides a water-based two-component mid-coat paint, which is composed of component A and component B in a mass ratio of 6:0.6 to 6:1.9; wherein

[0007] The component A comprises the following raw material components in percentage by mass: 30% to 35% of aqueous hydroxyl-containing acrylate dispersion, 3% to 10% of aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50°C, 0 to 10% of aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C, 0.2% to 1% of a first surfactant, 0.2% to 1% of a first defoamer, 0.2% to 1% of a substrate wetting agent, 0.1% to 1% of a leveling agent, 40% to 60% of an aqueous color paste, 3% to 6% of a first cosolvent, 1% to 3% of a neutralizer, 0.2% to 0.6% of a thickener, and 2% to 5% of water;

[0008] The hydroxyl content of the aqueous hydroxyl-containing acrylate dispersion is 3.5% to 4.5%, and the solid content of the aqueous hydroxyl-containing acrylate dispersion is 40% to 50%; the aqueous color paste comprises water, a dispersant, a second defoamer, a second surfactant, a pigment, a filler, a color paste stabilizer and a neutralizer;

[0009] The B component includes the following raw material components in percentage by mass: 70% to 80% of a curing agent and 20% to 30% of a second co-solvent; the curing agent is at least one of hexamethylene diisocyanate or a hydrophilic aliphatic polyisocyanate.

[0010] Compared with the prior art, the water-based two-component mid-coat paint provided by the present invention has component A as the main paint component and component B as the curing component; component A uses a water-based hydroxyl-containing acrylate dispersion and a water-based polycarbonate-containing aliphatic anionic polyurethane dispersion with a high glass transition temperature for compounding as a film-forming resin, and selectively adds a water-based aliphatic anionic polyurethane dispersion with a low glass transition temperature, and each film-forming resin has good compatibility. Through a specific ratio and the synergistic effect of each component, the characteristics of different types of water-based resins are brought into the best state, so that the coating film of the final water-based two-component mid-coat paint has excellent leveling, stone impact resistance, chemical resistance and weather resistance, and the gloss (60°) is 60-80, which is convenient for checking the paint film such as pinholes, flatness, etc., improves the inspection efficiency, ensures the accuracy of the inspection, and thus reduces the accident risk of rail transit vehicles. In addition, the coating film does not need to be polished when used in conjunction with the primer coating and the topcoat, and the interlayer adhesion is excellent, which can reach level 0. In the 3C1B process, the film thickness of the mid-coat is relatively thin (17μm to 23μm), which will cause the mid-coat to not cover the surface roughness of the electrophoretic paint sufficiently and cause the orange peel problem. The present invention introduces high-solid resin and high-solid clear varnish into the mid-coat (and topcoat) to reduce the shrinkage between the coatings to solve the orange peel problem. As for the problem of poor stone impact resistance that is prone to occur in composite coatings, the present invention introduces a resin with good toughness into the mid-coat and designs a mid-coat with decomposition impact energy to reduce the probability of broken stones hitting the substrate, while improving the hardness of the mid-coat, improving the adhesion between the mid-coat and the electrophoretic layer, and reducing the degree of peeling between the electrophoretic layer and the mid-coat. Even when large-scale construction is carried out under high temperature, low temperature or high humidity weather, the paint film joints of the water-based two-component mid-coat provided by the present invention have a smooth transition, no sagging or fly ash when sprayed, no overlap or marks, and the overall surface of the paint film is flat and smooth. At the same time, it can also balance the flexibility and hardness of the cured film, further fill and correct the surface of the workpiece that has been coated with primer, and can fully meet the needs of large-area spraying of the entire body of rail transit vehicles.

[0011] The paint film prepared by the waterborne polyurethane dispersion is soft, has good thixotropic index and anti-sagging properties, and has a moderate drying speed; at the same time, the permeability is very good, and different spraying technologies have little effect on the workability of the two-component mid-coat paint, the coating efficiency is high, the covering power is strong, and the bonding force with the upper and lower layers is also strong, which can ensure good interlayer adhesion. The flexibility of the molecular chain is the most important factor determining the glass transition temperature (Tg, referred to as the glass transition temperature) of the polymer. The better the flexibility of the main chain, the lower the glass transition temperature. The present invention has found through a large number of experiments that the waterborne polyurethane dispersion with a low glass transition temperature can still maintain good flexibility under low temperature conditions, and can improve the film-forming property under low temperature conditions; the waterborne polyurethane dispersion with a high glass transition temperature can improve the adaptability of the coating under high temperature environments and enhance its high temperature resistance; the waterborne polyurethane dispersions with different glass transition temperatures are compounded to adapt to and improve the workability of the paint film under various complex conditions such as high temperature and low temperature, and can form a smooth and bright coating.

[0012] In addition, the water-based hydroxyl-containing acrylate dispersion is a secondary dispersion with the characteristics of high solid content (40% to 50%), high hydroxyl content (3.5% to 4.5%) and low volatile organic compound content. The use of water-based hydroxyl-containing acrylate dispersion and polyisocyanate curing agent in two-component mid-coat paint has excellent reactivity and film-forming properties, which can make the two-component mid-coat paint have good adhesion, durability, water resistance, solvent resistance and thermal stability, improve the flexibility and hardness of the coating, and make the coating have high gloss, high fullness and high distinctness. Compared with low-hydroxyl acrylic resin, the hydroxyl value of water-based hydroxyl-containing acrylate dispersion is higher, and the number of hydroxyl groups in the film-forming resin will also increase accordingly, thereby improving the reactivity of the resin, so that the cross-linking speed and degree of cross-linking of the film-forming resin are significantly improved during curing. Due to the shortcomings of water-based hydroxyl-containing acrylate dispersions, such as fast drying, fast shrinkage of the paint film, many pits in the paint film, and obvious particles, it is difficult to match the gun during spraying (the overlap or connection of each spraying of different areas), and there is a phenomenon that one side is being sprayed while the other side has dried. Therefore, using only water-based hydroxyl-containing acrylate dispersions as film-forming resins cannot meet the requirements of large-area spraying of rail transit vehicle bodies. Compounding a specific proportion of water-based hydroxyl-containing acrylate dispersions in a hydroxyl-free water-based polyurethane dispersion can further enhance the adhesion of the paint film through chemical cross-linking of hydroxyl (-OH) and isocyanate (-NCO) curing agent; the synergistic effect of water-based polyurethane dispersions and water-based hydroxyl-containing acrylate dispersions can make up for the shortcomings of each single film-forming resin (single water-based polyurethane dispersions have poor self-thickening properties, low solid content, and poor water resistance, heat resistance and gloss of the paint film; single water-based acrylic resin emulsions are hot and viscous, cold and brittle, have poor flexibility, and are not solvent-resistant).

[0013] The present invention obtains a water-based two-component mid-coat with excellent comprehensive performance through the synergistic effect of each raw material component and a specific proportion content. The results of the embodiments show that the water-based two-component mid-coat provided by the present invention can be constructed on a large area under high temperature, low temperature or high humidity environment, and there is no need to polish the primer coating before the mid-coat is applied. After the mid-coat is applied and dried, it is free of polishing and can directly enter the construction process of the next topcoat. It has excellent interlayer adhesion between the previous primer layer and the next topcoat layer, and has excellent anti-sagging, color docking ability and interlayer adhesion without flying ash without affecting the construction fluidity. It also has excellent mechanical properties, and the appearance gloss of the paint film after the coating is completed is excellent, and it also has good polishing performance. The gloss disappears after polishing, which is convenient for checking the paint film such as pinholes, flatness, etc., improving the inspection efficiency, and ensuring the inspection accuracy, thereby reducing the accident risk of rail transit vehicles, and having high practical value and promotion value.

[0014] It should be noted that the hydroxyl content of the aqueous hydroxyl-containing acrylate dispersion is calculated based on the calculated value of the solid resin.

[0015] Preferably, the viscosity of the aqueous hydroxyl-containing acrylate dispersion is 1000 mPa·s to 3000 mPa·s.

[0016] Preferably, the solid content of the aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50° C. and the aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature ≤ 5° C. are both 33% to 42%.

[0017] Preferably, the aqueous hydroxyl-containing acrylate dispersion is at least one of Covestro Bayhydrol A 2470, Covestro Bayhydrol A 2770 or Covestro Bayhydrol A 2601.

[0018] Preferably, the aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion having a glass transition temperature of 40 to 50° C. is Bayhydrol UH 2606 produced by Covestro.

[0019] Preferably, the aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5° C. is at least one of Bayhydrol UH 2648 / 1, Bayhydrol UH 2110, Bayhydrol UH 2621 or Bayhydrol UH 2952 / 1.

[0020] In the present invention, the aliphatic anionic polyurethane dispersion has the advantages of light color, high transparency, good compatibility, slightly slow drying speed, softer paint film, moderate film volume shrinkage, strong corrosion resistance and strong interlayer adhesion, etc., which can minimize the phenomenon that one side is sprayed while the other side is already dry during large-area construction, reduce the number of pits in the paint film, and do not fly ash. After film formation, it has excellent leveling, chemical resistance and weather resistance, and has high toughness and good elasticity. Among them, the water-based aliphatic anionic polyurethane dispersion with a low glass transition temperature (especially Covestro Bayhydrol UH 2952 / 1) and the water-based polycarbonate-containing aliphatic anionic polyurethane dispersion with a high glass transition temperature (Covestro Bayhydrol UH 2606) can be attached to the body surface (or OEM product surface) without polishing, and have excellent adhesion and chemical resistance, which can not only meet the needs of large-area spraying of the whole body of rail transit vehicles, but also cooperate well with primer and topcoat coating. The water-based hydroxyl-containing acrylate dispersion has a high content of hydroxyl groups in the molecules, fewer chemical bonds between molecules, and a more orderly arrangement between molecules, resulting in a lower viscosity; in addition, the higher the hydroxyl value, the better the reaction activity with the polyisocyanate curing agent, the greater the crosslinking density, and the better the adhesion and hardness after film formation. Adding a certain amount of high hydroxyl value resin to the film-forming resin and compounding it with the water-based polyurethane dispersion can not only improve the thixotropic index and anti-sagging properties of the coating, but also synergistically improve the flexibility and hardness of the coating, so that the coating has high gloss, high fullness, and excellent water resistance, solvent resistance and thermal stability.

[0021] Preferably, the pigment includes organic pigment and inorganic pigment.

[0022] Preferably, the filler includes a soft filler and a hard filler.

[0023] Preferably, based on 100% of component A, the aqueous color paste includes 8.5% to 12.5% ​​of water, 1.5% to 2.5% of dispersant, 0.2% to 0.5% of a second defoamer, 0.2% to 0.8% of a second surfactant, 8% to 10% of an inorganic pigment, 0.1% to 0.3% of an organic pigment, 10% to 15% of a soft filler, 10% to 15% of a hard filler, 1.4% to 2.8% of a color paste stabilizer and 0.1% to 0.3% of a neutralizer.

[0024] Preferably, the dispersant is at least one of a nonionic wetting dispersant or an anionic wetting dispersant.

[0025] Further preferably, the nonionic wetting and dispersing agent is at least one of BYK DISPERBYK-190, BYK DISPERBYK-LPN 23160, BYK DISPERBYK-2010, BYK DISPERBYK-2012, allnex VXW6208-60 or BASF DispexUltra PX 4585.

[0026] Further preferably, the anionic wetting and dispersing agent is at least one of TEGO Dispers 747W, TEGO Dispers 757W, TEGO Dispers 750W or TEGO Dispers 755W.

[0027] Further preferably, the dispersant comprises a nonionic wetting dispersant and an anionic wetting dispersant in a mass ratio of 1:1 to 2:1.

[0028] Preferably, the mass ratio of the non-volatile matter of the dispersant to the organic pigment is 0.02:1 to 0.2:1.

[0029] Preferably, the mass ratio of the non-volatile matter of the dispersant to the inorganic pigment is 0.03:1 to 0.05:1.

[0030] Preferably, the second defoaming agent is at least one of BYK-011, BYK-024, BYK-1711, TEGO-810 or TEGO Airex 901W.

[0031] Preferably, the second surfactant is at least one of an acetylenic glycol surfactant or an alcohol alkoxy compound.

[0032] More preferably, the second surfactant is at least one of Surfynol AD01, Surfynol 440, Surfynol 104BC or BYK-DYNWET 800.

[0033] In the present invention, Surfynol AD01 is a Gemini acetylene glycol surfactant, HLB value (hydrophile-lipophile balance) = 4, has defoaming and wetting functions, can provide defoaming, dynamic wetting and help film-forming effects; Surfynol 440 is a nonionic acetylene glycol ethoxy compound, has low dynamic tension, good compatibility, HLB value = 8, has Gemini wetting and low foaming effects, can reduce the dynamic and static surface tension of the system, and prevent the occurrence of shrinkage holes, pinholes and fish eyes; Surfynol 104BC is a Gemini tetramethyldecynediol nonionic surfactant, has wetting, leveling, defoaming and other functions; BYK-DYNWET 800 is an alcohol alkoxy compound, has a slight foam stabilizing function, can reduce the dynamic surface tension of the system, and is particularly suitable for high-speed construction grinding slurry.

[0034] More preferably, the inorganic pigment is rutile titanium dioxide. More preferably, the inorganic pigment is DuPont R706.

[0035] More preferably, the organic pigment is high-pigment carbon black. More preferably, the organic pigment is at least one of PowCarbon2410G or Orion Carbon Black FW255FW255.

[0036] More preferably, the soft filler is at least one of talc or kaolin.

[0037] Further preferably, the hard filler is at least one of barite powder, ultrafine precipitated barium sulfate or heavy calcium.

[0038] For example, the particle sizes of the soft filler and the hard filler are both 1200-1300 meshes.

[0039] Preferably, the color paste stabilizer includes at least three of water-based fumed silica, organically modified montmorillonite clay rheological additives, modified urea rheological additives, resin-free color paste moisturizers or anti-drying agents for water-based pigment concentrates.

[0040] Further preferably, the color paste stabilizer includes at least three of Degussa AEROSIL R972, Deqian BENTONE LT, BYK RHEOBYK-420, BYK RHEOBYK-425, TEGO Humectant 7005 or BYKETOL-PC.

[0041] More preferably, the color paste stabilizer includes Degussa AEROSIL R972, Deqian BENTONE LT and TEGO Humectant 7005 in a mass ratio of 2:1:8 to 3:1:12.

[0042] More preferably, the color paste stabilizer includes Degussa AEROSIL R972, BYK RHEOBYK-420 and BYKETOL-PC in a mass ratio of 2:1:8 to 3:1:12.

[0043] In the present invention, AEROSILR972 is a water-based fumed silica, which contains silanol groups on the surface. After being fully stirred and dispersed, hydrogen bonds are formed between the silanol groups to produce a three-dimensional network structure, thereby increasing the viscosity of the dispersion system, producing thixotropic flow properties, playing an anti-settling role, and improving the stability, corrosion resistance and thixotropy of the pigment; BENTONE LT is an organically modified montmorillonite clay rheological additive, which has the functions of anti-settling, thickening, excellent thermal stability of viscosity and improving the stability of the coating. The coating is not prone to stratification, precipitation and the like, and can produce excellent thixotropic effects, prolong the open time of the coating film, which is conducive to the actual drying of the paint film, and the paint film surface is not dried too quickly, resulting in the water vapor in the paint film not being able to come out (not prone to blistering), and the construction performance is good, and the adhesion, corrosion resistance and antifouling properties of the coating are also improved; RHEOBYK-420 is a modified urea rheological additive, which has anti-settling and anti-sagging effects and can produce a thixotropic effect; TEGO Humectant 7005 is a resin-free color paste moisturizer; BYKETOL-PC is an anti-drying agent for water-based pigment concentrates and is also a solution of modified urea. Based on a specific molecular structure, it can optimally control water evaporation and ensure that the water-based pigment concentrate does not dry out too quickly.

[0044] Preferably, the neutralizing agent is an 8 wt % to 12 wt % aqueous solution of dimethylethanolamine.

[0045] Preferably, the method for preparing the water-based color paste comprises the following steps:

[0046] Add the dispersant, the second defoamer and the second surfactant into water, mix them evenly, add the pigment, filler and color paste stabilizer, grind them, add the neutralizer to obtain the water-based color paste.

[0047] For example, the preparation method of the water-based color paste comprises the following steps:

[0048] Add water to a clean container, stir at 280rpm-320rpm, add dispersant and second defoamer in sequence, adjust the speed to 800rpm-1500rpm, add second surfactant, stir for 5min-10min to make it uniform; adjust the speed to 1500rpm-2000rpm, add pigment, filler and color paste stabilizer in sequence, adjust the speed to 2000rpm-3000rpm, disperse and stir for 25min-40min; grind with horizontal grinder or basket grinder; finally add neutralizer, mix well to obtain water-based color paste.

[0049] Since the second surfactant has low solubility in water (such as Surfynol AD01's HLB=4, solubility in water is 0.1%), low molecular weight, and is volatile, in order to fully adsorb it onto various particles in the system to achieve good compatibility, it needs to be fully dispersed. It is recommended that the dispersion speed be no less than 800rpm to avoid water sensitivity problems.

[0050] More preferably, the pH of the aqueous color paste is 8 to 8.5.

[0051] More preferably, the fineness of the water-based color paste is 20 μm to 30 μm.

[0052] It should be noted that the color paste stabilizer is not added after compounding and premixing, but after all the pigments and fillers in the color paste are added and dispersed evenly at high speed, the color paste stabilizer is added in sequence, and dispersed evenly at high speed after adding. In the present invention, the color paste stabilizer (such as Degussa AEROSIL R972, Deqian BENTONE LT) should be well dispersed together with the pigment to effectively play its corresponding role, thereby achieving the most ideal dispersion degree and improving processing efficiency. If a compounding method is adopted (first mixing all the raw materials of the color paste stabilizer and then adding the whole to the water-based color paste system), an uneven gel phenomenon will occur, thereby reducing the use efficiency of the color paste stabilizer.

[0053] In addition, there is no need to adjust the pH before and during grinding, and no other components such as resins, amines, organic co-solvents, thickeners, etc. are added, otherwise the grinding effect of the pigment slurry will be affected.

[0054] Preferably, the first surfactant is a gemini acetylenic diol surfactant.

[0055] Further preferably, the first surfactant is at least one of Surfynol AD01, Surfynol 104BC or Surfynol 440 manufactured by Air Chemicals.

[0056] More preferably, the first surfactant is at least two of Surfynol AD01, Surfynol 104BC or Surfynol 440.

[0057] For example, the first surfactant is Surfynol AD01, Surfynol 104BC and Surfynol 440 of Air Chemicals in a mass ratio of 2:1:1.

[0058] In the present invention, Surfynol AD01 is a Gemini acetylene glycol surfactant, HLB value (hydrophile-lipophile balance) = 4, has defoaming and wetting functions, can provide defoaming, dynamic wetting and help film formation effects; Surfynol 104BC is a Gemini tetramethyldecynediol nonionic surfactant, the dynamic surface tension of the wet film is slightly lower than the surface tension of the substrate, can well wet the substrate, form a continuous and stable paint film, has low water sensitivity, has wetting, leveling, defoaming, improves dispersibility, reduces surface tension and stabilizes consistency and viscosity and other functions; Surfynol 440 is a nonionic acetylene glycol ethoxylate, low dynamic tension, good compatibility, HLB value = 8, has Gemini wetting and low foaming effects, can reduce the dynamic and static surface tension of the system, and prevent the occurrence of shrinkage holes, pinholes and fish eyes.

[0059] Preferably, the first defoaming agent is at least one of BYK-093, BYK-011, BYK-0381, TEGO-830 or TEGO Airex 901W.

[0060] Preferably, the substrate wetting agent is a polyether-modified silicone surfactant.

[0061] Further preferably, the substrate wetting agent is at least one of BYK-345, BYK-346, BYK-347, Tego-4100, Tego-280 or Surfynol 104BC.

[0062] The preferred substrate wetting agent of the present invention can effectively reduce the surface tension of the system, significantly improve the substrate wettability of the system, and at the same time has good recoatability without increasing the surface smoothness, and is suitable for all water-based systems without cosolvents.

[0063] Preferably, the leveling agent is at least one of BYK-378, BYK-381, BYK-333, BYK-331, Tego-4100 or Surfynol 104BC.

[0064] The paint molecules are constantly moving during the leveling process. As the viscosity of the paint gradually increases during the leveling process, the system molecules gradually form Bénard vortices, which leads to defects such as pinholes and sagging in the film-forming process. Among the preferred leveling agents of the present invention, BYK-378 is a polyether-modified dimethyl polysiloxane, which can significantly reduce the surface tension of the system, improve the surface smoothness, and thus improve the anti-scratch performance of the paint. It also has excellent substrate wettability and good anti-shrinkage effect, and has a good effect even at a low addition amount. It also has low foam stability, good compatibility, and is easy to recoat without causing oil spots; BYK-381 is an ionic polyacrylate solution type surface additive, which can improve the leveling and substrate wettability of the system and prevent surface defects (shrinkage and pinholes); Tego-4100 is a leveling agent with a twin structure, which has high activity and unstable foam. Even at extremely low concentrations, it can effectively reduce surface tension and improve wettability and leveling performance.

[0065] The dynamic surface tension of the wet film needs to be slightly lower than the surface tension of the substrate, so that the paint film can wet the substrate well and form a continuous and stable paint film. The preferred surfactants, substrate wetting agents and leveling agents of the present invention have low water sensitivity, which can effectively reduce the surface tension and achieve a balance between static and dynamic surface tensions. The special structure enables it to have wetting and defoaming effects, which can improve the dispersibility of the system, improve fluidity and leveling, control foam, and stabilize consistency and viscosity.

[0066] Preferably, the first co-solvent includes at least three of propylene glycol methyl ether propionate, propylene glycol butyl ether, dipropylene glycol dimethyl ether, ethylene glycol butyl ether, dipropylene glycol methyl ether, dimethyl sulfoxide, N-methylpyrrolidone, dipropylene glycol butyl ether or diethylene glycol monobutyl ether.

[0067] Further preferably, based on the A component as 100%, the first co-solvent includes 1% to 2% of a first solvent, 0.75% to 1.5% of a second solvent and 1.25% to 2.5% of a third solvent; the first solvent includes at least one of propylene glycol methyl ether propionate (PMP), dipropylene glycol dimethyl ether (DMM) or propylene glycol butyl ether (PNB), the second solvent includes at least one of ethylene glycol butyl ether (BCS), dipropylene glycol methyl ether (DPM) or dimethyl sulfoxide (DMSO), and the third solvent includes at least one of N-methylpyrrolidone (NMP), diethylene glycol monobutyl ether (BDG) or dipropylene glycol butyl ether (DPNB).

[0068] More preferably, the first co-solvent comprises propylene glycol methyl ether propionate (PMP), dipropylene glycol methyl ether (DPM) and N-methylpyrrolidone (NMP) in a mass ratio of 1:1:1.

[0069] More preferably, the first co-solvent comprises propylene glycol methyl ether propionate (PMP), propylene glycol butyl ether (PNB), ethylene glycol butyl ether (BCS), dipropylene glycol methyl ether (DPM), N-methylpyrrolidone (NMP) and dipropylene glycol butyl ether (DPNB) in a mass ratio of 1.5:0.5:0.5:1:1.5:1.

[0070] More preferably, the first co-solvent comprises propylene glycol butyl ether (PNB), dipropylene glycol dimethyl ether (DMM), ethylene glycol butyl ether (BCS), dipropylene glycol methyl ether (DPM), N-methylpyrrolidone (NMP) and dipropylene glycol butyl ether (DPNB) in a mass ratio of 1.5:0.5:0.5:1:1.5:1.

[0071] The present invention controls the boiling point (gradient boiling point) and solubility of the first cosolvent miscible with water (including the solubility of the solvent in water and the solubility of water in the solvent), which is beneficial to balancing the volatilization rate during the film-forming process, improving the solubility in water, and is more conducive to coating the paint film under high temperature or high humidity, with a moderate drying speed, no fly ash, no sagging, and no obvious traces of grabbing. As long as the ventilation conditions on site are good, normal coating can be performed. The specific first cosolvent can couple different phases, has a strong solubility for both polar and non-polar substances, interacts with the solution system in the water-based paint, causes it to produce a slight phase separation, helps to reduce the surface tension of the water-based system, enhances the fluidity of the paint, thereby adjusting its paint performance, increasing the viscosity of the water-based paint, changing the drying time of the paint, improving the wettability and coating effect of the paint, and improving the elasticity, wear resistance, water resistance, solvent resistance and mechanical strength of the paint film. The preferred first co-solvent can also be used as a film-forming aid. Its unique hydrophilic and lipophilic balance properties enable it to exert different film-forming effects on different resins, helping the coating to form a uniform and smooth coating. In particular, it can significantly reduce the surface tension of the system, assist in leveling, and prevent cracking and orange peel.

[0072] Preferably, the thickener is a polyurethane associative thickener.

[0073] Further preferably, the thickener is at least one of Hemmings RHEOLATE 299, BYK OPTIFLO-H 6000VF, BYK RHEOBYK-H 7625VF, Rohm and Haas RM5000 or Rohm and Haas RM-8W.

[0074] More preferably, the thickener is at least two of Hemmings RHEOLATE 299, BYK OPTIFLO-H 6000VF, BYK RHEOBYK-H7625VF, Rohm and Haas RM5000 or Rohm and Haas RM-8W.

[0075] In the present invention, RHEOLATE 299, OPTIFLO-H 6000VF, RHEOBYK-H 7625VF and RM5000 are the same type of polyurethane associative thickeners, which are not affected by pH value; RHEOLATE 299 can provide efficient thickening in the medium and low shear rate range, OPTIFLO-H 6000VF and RHEOBYK-H 7625VF can sharply increase the viscosity under low shear, and have excellent leveling and anti-splashing properties, RM5000 can increase the viscosity in the high shear rate range, and the four play a complementary role, which can prevent the sedimentation of the system and improve the water resistance and the corrosion resistance; RM-8W is a low-odor, solvent-free hydrophobically modified polyurethane nonionic associative thickener, which has excellent flow and leveling properties, uniform film-forming properties, glossiness and high thickening efficiency.

[0076] Preferably, the solid content of component A is 45% to 60%. Further preferably, the solid content of component A is 48% to 57%.

[0077] In the present invention, the solid content of component A refers to the mass proportion of all solid components in component A (including resin dispersion, pigment and filler).

[0078] Preferably, the mass ratio of the component A to the component B is 6:0.7 to 6:1.7, and more preferably 6:0.8 to 6:1.1.

[0079] Preferably, based on 100% of the B component, the curing agent includes 25% to 30% of low-viscosity hydrophobic hexamethylene diisocyanate, 25% to 30% of high-viscosity hydrophilic hexamethylene diisocyanate and 18% to 22% of hydrophilic modified isophorone diisocyanate.

[0080] It should be noted that the hydrophilic modified isophorone diisocyanate in the present invention refers to a hydrophilic modified aliphatic polyisocyanate based on isophorone diisocyanate (IPDI).

[0081] Further preferably, the low-viscosity hydrophobic hexamethylene diisocyanate is at least one of Covestro Desmodur N3900, Covestro Desmodur N3600 or Wanhua WANNATE HT-600.

[0082] Further preferably, the high-viscosity hydrophilic hexamethylene diisocyanate is at least one of Bayhydrol XP2655, Bayhydur XP 2547, Bayhydur XP 2487 / 1, Bayhydur 304 or Bayhydur 305.

[0083] Preferably, the solid content of the hydrophilic aliphatic polyisocyanate is 60% to 70%.

[0084] Preferably, the -NCO content of the hydrophilic aliphatic polyisocyanate is 8.5% to 12%.

[0085] Further preferably, the hydrophilic aliphatic polyisocyanate is at least one of Covestro Bayhydur 401-70, Covestro Bayhydur 401-60 or Evonik Vestanat T1890E.

[0086] The present invention can further enhance the curing effect and improve the construction fluidity, viscosity and glossiness of the coating by limiting the type of curing agent.

[0087] Preferably, the second co-solvent is at least two of propylene glycol methyl ether acetate (PMA), propylene glycol methyl ether acrylate (PMP), propylene glycol diacetate (PGDA), ethylene glycol butyl ether acetate (BGA), dipropylene glycol dimethyl ether (DMM), propylene carbonate (PC) or dibasic acid ester (DBE).

[0088] Further preferably, based on 100% of the B component, the second co-solvent includes 6% to 9% of a fourth solvent, 8% to 12% of a fifth solvent and 6% to 9% of a sixth solvent; the fourth solvent includes at least one of propylene glycol methyl ether acetate (PMA) or propylene glycol methyl ether propionate (PMP), the fifth solvent includes at least one of propylene glycol diacetate (PGDA), ethylene glycol butyl acetate (BGA) or dipropylene glycol dimethyl ether (DMM), and the sixth solvent includes at least one of propylene carbonate (PC) or dibasic acid ester (DBE).

[0089] Table 1 Summary of the physicochemical properties of the second co-solvent

[0090]

[0091] In the present invention, a certain amount of the second cosolvent is added to the curing component, which can not only improve the compatibility of the curing agent with the aqueous hydroxyl-containing acrylate dispersion, but also prolong the open time of the paint film, which is beneficial to leveling. The specific second co-solvents are all environmentally friendly solvents (see Table 1 for specific properties) with the following characteristics: (1) They contain multiple functional groups and have strong solubility for both polar and non-polar substances, which can improve the strength of the coating film; (2) They have low surface tension, strong solvent power, low viscosity and good volatility, which can provide good solubility and fluidity, ensure uniform coating and easy construction, and at the same time improve the adhesion and durability of the coating, adjust the volatilization rate of the entire system, adjust the drying speed of the paint film, reduce pinholes and fish eyes, and increase gloss, wetting, leveling and re-leveling; (3) Propylene carbonate has good film-forming properties and strong carbon dioxide absorption capacity. When used with a hydrophilic isocyanate curing agent, the effect is excellent, which can improve prickly heat and reduce bubbles; (4) The use of multiple second co-solvents can complement each other to achieve a better comprehensive effect. In addition, by compounding second co-solvents with different boiling points (gradient boiling points), it is beneficial to balance the volatilization rate during the film-forming process and improve the solubility in water. For example, the synergy of propylene glycol methyl ether propionate (PMP), propylene glycol diacetate (PGDA), and propylene carbonate (PC) can not only improve the strength of the coating film, but also facilitate the stable storage of the coating. It can also absorb carbon dioxide during the coating and film-forming process, and is extremely effective in diluting water-based isocyanate curing agents.

[0092] Preferably, the molar ratio of -NCO in the B component to -OH in the A component is 1.3:1 to 1.5:1, and more preferably 1.3:1 to 1.4:1.

[0093] The preferred molar ratio of -NCO to -OH of the present invention can not only meet the combined application of component A and component B, but also after adding a specific activated diluent during the subsequent use, the ratio of -NCO to -OH in the system is more conducive to the formation of a paint film. The amount of curing agent is too much, and the second cosolvent in component B is also increased, resulting in the relative need to extend the surface drying time of the system, which is not conducive to the rhythm of on-site construction. At the same time, excessive curing agent also leads to a high cross-linking density of the coating film, too high hardness, and decreased flexibility and impact resistance; and, with the increase of n(-NCO) / n(-OH), the bubble-free film thickness of the coating film decreases, and excessive -NCO increases the probability of side reactions with water, and the generated CO2 is retained in the coating film. As the degree of curing increases, bubbles are easily generated on the surface of the coating film, thereby affecting the appearance and performance of the topcoat coating film.

[0094] In a second aspect, the present invention provides a method for preparing a water-based two-component mid-coat paint, comprising the following steps:

[0095] S1, weighing each raw material according to the designed ratio, adding an aqueous hydroxyl-containing acrylate dispersion, an aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50°C, and an aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C into water, mixing evenly, adding a first surfactant, a first defoamer, a substrate wetting agent, a leveling agent, an aqueous color paste, and a first cosolvent, mixing evenly, and then sequentially adding a neutralizer and a thickener, mixing evenly, to obtain component A;

[0096] S2, adding the second co-solvent into the curing agent, mixing evenly, to obtain component B.

[0097] It should be noted that there is no order of precedence for steps S1 and S2.

[0098] The preparation method of the water-based two-component mid-coat provided by the invention does not require special treatment of the raw materials and is simple and easy to implement.

[0099] For example, the preparation method of component A comprises the following steps:

[0100] Weigh the raw materials according to the designed ratio, add the aqueous hydroxyl-containing acrylate dispersion, the aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50°C, and the aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C into a clean container, add water at 600 rpm to 800 rpm, and stir for 4 to 6 minutes; then add the first surfactant, the first defoamer, the substrate wetting agent, the leveling agent, the aqueous color paste and the first cosolvent in sequence, and continue to stir at 600 rpm to 800 rpm for 10 to 15 minutes; then add the neutralizer to adjust the pH of the system to 8 to 8.5; finally add the thickener, mix well, and obtain component A.

[0101] In a third aspect, the present invention provides the use of the above-mentioned water-based two-component mid-coat in automotive coatings.

[0102] Preferably, the vehicle coating is a coating for rail transit vehicles.

[0103] In a fourth aspect, the present invention provides a method for using the above-mentioned water-based two-component mid-coat paint, comprising the following steps:

[0104] Mix component A and component B evenly, add activation diluent, mix evenly to obtain construction coating, and evenly apply it on the mid-coat paint;

[0105] The activated diluent comprises an aqueous hydroxyl-containing acrylate dispersion, an aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50° C., an aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5° C., a water-based synthetic sheet silicate solution, a water-based modified urea solution, a first cosolvent, a stabilizer, a first defoamer, a leveling agent and water.

[0106] In the method of using a water-based two-component mid-coat, a unique activated diluent is used to dilute the water-based two-component mid-coat (component A + component B), which has the following beneficial effects: (1) improving the system's tolerance to high levels of surfactants or extreme pH values; (2) preventing the coating from sagging or miscibility; and (3) accelerating the formation of the structure after construction during large-area spraying, thereby improving the adhesion of vertical surfaces (improving the interlayer adhesion between the water-based mid-coat and the primer and topcoat).

[0107] Preferably, the activated diluent comprises the following raw material components in percentage by mass: 8% to 11.5% of aqueous hydroxyl-containing acrylate dispersion, 3% to 4.5% of aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50°C, 3% to 4.5% of aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature ≤ 5°C, 25% to 33.5% of water-based synthetic sheet silicate solution, 0.5% to 0.7% of water-based modified urea solution, 7.5% to 8.5% of a first cosolvent, 7.5% to 8.5% of a stabilizer, 0.5% to 0.7% of a first defoamer, 0.5% to 0.7% of a leveling agent and 27% to 42% of water, and the sum of each component is 100%.

[0108] Preferably, the mass ratio of the component A to the activated diluent is 100:(20-30).

[0109] The present invention adopts the above mass ratio to ensure the solid content of the construction coating. The specific amount of the activated diluent can be adjusted according to the ambient temperature and humidity and whether the construction spraying sags. Generally, the higher the temperature or humidity, the more the activated diluent is added; the more serious the sag phenomenon, the more the activated diluent is added.

[0110] Preferably, the hydroxyl content of the aqueous hydroxyl-containing acrylate dispersion is 3.5% to 4.5%.

[0111] Preferably, the viscosity of the aqueous hydroxyl-containing acrylate dispersion is 1000 mPa·s to 3000 mPa·s.

[0112] Preferably, the solid content of the aqueous hydroxyl-containing acrylate dispersion is 40% to 50%.

[0113] Preferably, the solid content of the aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50° C. and the aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature ≤ 5° C. are both 33% to 42%.

[0114] Preferably, the aqueous hydroxyl-containing acrylate dispersion is at least one of Covestro Bayhydrol A 2470, Covestro Bayhydrol A 2770 or Covestro Bayhydrol A 2601.

[0115] Preferably, the aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion having a glass transition temperature of 40 to 50° C. is Bayhydrol UH 2606 produced by Covestro.

[0116] Preferably, the aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5° C. is at least one of Bayhydrol UH 2648 / 1, Bayhydrol UH 2110, Bayhydrol UH 2621 or Bayhydrol UH 2952 / 1.

[0117] Preferably, the water-based synthetic sheet silicate solution comprises the following raw material components in percentage by mass: 1.5% to 2.5% of organic modified synthetic layer silicate, 1.5% to 2.5% of emulsifying dispersant and 95% to 97% of water, and the sum of the components is 100%.

[0118] More preferably, the organic-modified synthetic layered silicate is at least one of BYK Laponite-RD or BYK Laponite-RDS.

[0119] Laponite-RD and Laponite-RDS are synthetic sheet silicates that are insoluble in water but can hydrate and swell in water to form a colorless and transparent colloid. When the concentration in water is above 2%, a colloid with improved thixotropy can be formed, which plays an activation and regulating role in anti-sagging. The present invention utilizes the synergistic effect of the compounding of LAPONITE and polymer to improve the tolerance of the system to high content of surfactants, electrolytes or extreme pH values.

[0120] Further preferably, the emulsifying dispersant is at least one of polyethylene glycol and polypropylene glycol. If the emulsifying dispersant includes polyethylene glycol and polypropylene glycol, the mass ratio of polyethylene glycol to polypropylene glycol may be 1:1.

[0121] More preferably, the emulsifying dispersant is at least one of PEG-1000, PEG-1500, PPG-200, PPG-400 or PPG-600.

[0122] Preferably, the method for preparing the water-based synthetic sheet silicate solution comprises the following steps:

[0123] The emulsifying dispersant is added into water and mixed evenly, and then the organic modified synthetic layered silicate is added and mixed evenly to obtain a water-based synthetic sheet silicate solution.

[0124] For example, under stirring at 400 rpm to 600 rpm, an emulsifying dispersant is added to water, the rotation speed is adjusted to 1000 rpm to 1500 rpm, and the organic modified synthetic layered silicate is slowly added, and stirring is continued until the solution is clear and no dissolved particles are seen, thereby obtaining a water-based synthetic sheet silicate solution.

[0125] Preferably, the water-based modified urea solution is at least one of BYK RHEOBYK-7420CA, BYK RHEOBYK-7420ET or BYK RHEOBYK-7420ES.

[0126] In the present invention, the water-based modified urea solution is a liquid rheological agent, and a specific amount of the water-based modified urea solution can produce a strong thixotropic effect, thereby improving the anti-settling and anti-sagging properties of the system.

[0127] Preferably, the first co-solvent includes at least three of propylene glycol methyl ether propionate, propylene glycol butyl ether, dipropylene glycol dimethyl ether, ethylene glycol butyl ether, dipropylene glycol methyl ether, dimethyl sulfoxide, N-methylpyrrolidone, dipropylene glycol butyl ether or diethylene glycol monobutyl ether.

[0128] Further preferably, based on the A component as 100%, the first co-solvent includes 1% to 2% of a first solvent, 0.75% to 1.5% of a second solvent and 1.25% to 2.5% of a third solvent; the first solvent includes at least one of propylene glycol methyl ether propionate (PMP), dipropylene glycol dimethyl ether (DMM) or propylene glycol butyl ether (PNB), the second solvent includes at least one of ethylene glycol butyl ether (BCS), dipropylene glycol methyl ether (DPM) or dimethyl sulfoxide (DMSO), and the third solvent includes at least one of N-methylpyrrolidone (NMP), diethylene glycol monobutyl ether (BDG) or dipropylene glycol butyl ether (DPNB).

[0129] Preferably, the stabilizer is at least one of propylene glycol methyl ether acetate (PGMEA) or propylene glycol methyl ether propionate (PMP).

[0130] In the present invention, the preferred stabilizer can provide good solubility and fluidity, ensure uniform coating and easy construction, and improve the adhesion and durability of the coating.

[0131] Preferably, the first defoaming agent is at least one of BYK-093, BYK-011, BYK-0381, TEGO-830 or TEGO Airex 901W.

[0132] Preferably, the leveling agent is at least one of BYK-378, BYK-381, BYK-333, BYK-331, Tego-4100 or Surfynol 104BC.

[0133] For example, the preparation method of the activated diluent comprises the following steps:

[0134] Weigh the raw materials according to the designed ratio, add an aqueous hydroxyl-containing acrylate dispersion, an aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50°C, an aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C, a first defoamer, a leveling agent, a first cosolvent, a stabilizer, a water-based synthetic sheet silicate solution and a water-based modified urea solution into water at 400 rpm to 600 rpm, and continue stirring at 600 rpm to 800 rpm for 8 min to 12 min to obtain an activated diluent.

[0135] The corresponding film-forming resin in component A is added to the activated diluent of the present invention, which increases the solid content of the construction and the hydroxyl content, further promotes the reaction activity of the film-forming resin and the isocyanate curing agent, thereby enhancing the adhesion and improving the gloss, distinctness and fullness of the paint film; through the synergistic effect of compounding the aqueous hydroxyl-containing acrylate dispersion and the aqueous polyurethane dispersion with different glass transition temperatures, the tolerance of the system to the limit film thickness of the two-component mid-coat paint is improved, and an ideal paint film surface state can be formed after accelerated construction, which is particularly suitable for large-area construction spraying of rail transit vehicle bodies, and can be smoothly constructed under high temperature, low temperature or high humidity environments. The water-based modified urea solution is a liquid rheological agent that can produce a strong thixotropic effect and can improve the anti-settling and anti-sagging properties of water-based and high-polarity systems. In addition, the stabilizer is a high-grade industrial solvent with excellent performance. It has strong solubility and fluidity for both polar and non-polar substances, which can ensure uniform coating and easy construction, further improve the adhesion and durability of the coating, and at the same time improve the solubility of the water-based synthetic sheet silicate solution, ensuring that the coating can be stored for a long time without flocculation and agglomeration. During construction, by adding an activated diluent, the interlayer adhesion can be greatly improved and the rheological properties can be accurately adjusted, thereby improving the interlayer adhesion of the two-component mid-coat, primer, and topcoat.

[0136] The water-based synthetic sheet silicate solution and the water-based modified urea solution can form a synergistic effect, increase the low shear viscosity of the coating, prevent the coating from sagging or mixing during construction, improve the construction and storage stability of the coating, and effectively prevent the sedimentation and dehydration shrinkage of solid matter in the water-based coating system, thereby accelerating the formation of the structure after construction. The present invention has found through a large number of experiments that when the rheological additive water-based synthetic sheet silicate solution and the surfactant water-based modified urea solution are compounded, if the rheological additive is used in excessive amounts, it will cause the activation dilution to be unable to be stored for a long time (caking and flocculation will occur after long storage), and it will also cause the water resistance of the water-based two-component medium-coating to deteriorate; if the surfactant is used in excessive amounts, it will cause the paint film to have defects such as shrinkage cavities, prickly heat, and orange peel. Therefore, the rheological additive is compounded with the surface additive, stabilizer and other additives and part of the film-forming resin in a specific ratio, which further improves the storage stability and water resistance of the coating, and makes the appearance of the paint film reach the best state. DETAILED DESCRIPTION

[0137] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0138] The water used in the embodiments of the present invention is deionized water.

[0139] The test instrument used in the present invention comprises:

[0140] Grid marker, Guangzhou Biaogeda;

[0141] Pencil hardness tester, impact instrument, bending tester, cupping tester, distinctness of image tester, BYK, Germany;

[0142] MA85 multi-angle wind photometer, X-Rite, USA;

[0143] ISO No. 6 cup, Tu-4# cup, solvent resistance wiper, pH meter, film thickness meter, Shanghai Modern Environmental Engineering Technology Co., Ltd.;

[0144] Salt spray resistance test equipment, artificial weathering resistance (QUA / SPARY), Q-Lab, USA.

[0145] In order to better illustrate the present invention, further examples are given below.

[0146] Example 1

[0147] This embodiment provides a water-based two-component mid-coat paint, which is composed of component A and component B in a mass ratio of 6:0.9.

[0148] Component A is composed of the following raw material components in percentage by mass: 32% aqueous hydroxyl-containing acrylate dispersion, 5% aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40-50°C (denoted as PUD with Tg=40-50), 5% aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature ≤5°C (denoted as PUD with Tg≤5), 0.6% first surfactant, 0.6% first defoamer, 0.6% substrate wetting agent, 0.6% leveling agent, 46.2% aqueous color paste (including 9% water, 2% dispersant, 0.3% second defoamer, 0.5% second surfactant, 9% inorganic pigment, 0.2% organic pigment, 11.5% soft filler, 11.5% hard filler, 2% color paste stabilizer and 0.2% neutralizer), 4% first cosolvent, 2% neutralizer, 0.4% thickener and 3% water.

[0149] Component B is composed of the following raw material components in percentage by mass: 75% of curing agent (28% of low viscosity hydrophobic hexamethylene diisocyanate, 27% of high viscosity hydrophilic hexamethylene diisocyanate and 20% of hydrophilic modified isophorone diisocyanate) and 25% of the second cosolvent.

[0150] The specific components of the above raw materials are shown in Table 2. After calculation, the solid content of component A is 52.6%.

[0151] The preparation method of the above-mentioned water-based two-component mid-coat paint comprises the following steps:

[0152] S1, weigh the raw materials according to the designed ratio, add the aqueous hydroxyl-containing acrylate dispersion, the aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40-50°C, and the aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C into a clean container, add water at 700rpm, and stir for 5min; then add the first surfactant, the first defoamer, the substrate wetting agent, the leveling agent, the aqueous color paste and the first cosolvent in sequence, and continue to stir at 700rpm for 13min; then add the neutralizer to adjust the pH of the system to 8.5; finally add the thickener, mix well, and obtain component A.

[0153] S2, adding the second co-solvent into the curing agent, mixing evenly, to obtain component B.

[0154] Example 2

[0155] This embodiment provides a water-based two-component mid-coat paint, which is composed of component A and component B in a mass ratio of 6:0.9.

[0156] Component A is composed of the following raw material components in percentage by mass: 33% aqueous hydroxyl-containing acrylate dispersion, 3% aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50°C, 10% aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C, 0.2% first surfactant, 0.2% first defoamer, 0.2% substrate wetting agent, 0.1% leveling agent, 47.1% aqueous color paste (including 12.5% ​​water, 1.5% dispersant, 0.2% second defoamer, 0.2% second surfactant, 8% inorganic pigment, 0.1% organic pigment, 13.1% soft filler, 10% hard filler, 1.4% color paste stabilizer and 0.1% neutralizer), 3% first cosolvent, 1% neutralizer, 0.2% thickener and 2% water.

[0157] Component B is composed of the following raw material components in percentage by mass: 73% of curing agent (30% of low viscosity hydrophobic hexamethylene diisocyanate, 25% of high viscosity hydrophilic hexamethylene diisocyanate and 18% of hydrophilic modified isophorone diisocyanate) and 27% of the second cosolvent.

[0158] The specific components of the above raw materials are shown in Table 2. After calculation, the solid content of component A is 51.9%.

[0159] The preparation method of the above-mentioned water-based two-component mid-coat paint comprises the following steps:

[0160] S1, weigh the raw materials according to the designed ratio, add the aqueous hydroxyl-containing acrylate dispersion, the aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40-50°C, and the aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C into a clean container, add water at 800rpm, and stir for 4min; then add the first surfactant, the first defoamer, the substrate wetting agent, the leveling agent, the aqueous color paste and the first cosolvent in sequence, and continue to stir at 800rpm for 10min; then add the neutralizer to adjust the pH of the system to 8.5; finally add the thickener, mix well, and obtain component A.

[0161] S2 is the same as in Example 1 and will not be described in detail.

[0162] Example 3

[0163] This embodiment provides a water-based two-component mid-coat paint, which is composed of component A and component B in a mass ratio of 6:1.

[0164] Component A is composed of the following raw material components in percentage by mass: 35% aqueous hydroxyl acrylate dispersion, 9.5% aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50°C, 0.2% first surfactant, 0.2% first defoamer, 0.2% substrate wetting agent, 0.1% leveling agent, 40.2% aqueous color paste (including 8.5% water, 1.5% dispersant, 0.2% second defoamer, 0.2% second surfactant, 8% inorganic pigment, 0.3% organic pigment, 10% soft filler, 10% hard filler, 1.4% color paste stabilizer and 0.1% neutralizer), 6% first cosolvent, 3% neutralizer, 0.6% thickener and 5% water.

[0165] Component B is composed of the following raw material components in percentage by mass: 80% of curing agent (28% of low viscosity hydrophobic hexamethylene diisocyanate, 30% of high viscosity hydrophilic hexamethylene diisocyanate and 22% of hydrophilic modified isophorone diisocyanate) and 20% of the second cosolvent.

[0166] The specific components of the above raw materials are shown in Table 2. After calculation, the solid content of component A is 48.7%.

[0167] The preparation method of the above-mentioned water-based two-component mid-coat paint comprises the following steps:

[0168] S1, weigh the raw materials according to the designed ratio, add the aqueous hydroxyl-containing acrylate dispersion, the aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40-50°C, and the aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C into a clean container, add water at 600rpm, and stir for 6min; then add the first surfactant, the first defoamer, the substrate wetting agent, the leveling agent, the aqueous color paste and the first cosolvent in sequence, and continue to stir at 600rpm for 15min; then add the neutralizer to adjust the pH of the system to 8; finally add the thickener, mix well, and obtain component A.

[0169] S2 is the same as in Example 1 and will not be described in detail.

[0170] Example 4

[0171] This embodiment provides a water-based two-component mid-coat paint, which is composed of component A and component B in a mass ratio of 6:0.7.

[0172] Component A is composed of the following raw material components in percentage by mass: 30% aqueous hydroxyl-containing acrylate dispersion, 4% aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40-50°C, 4% aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature ≤5°C, 1% first surfactant, 1% first defoamer, 1% substrate wetting agent, 1% leveling agent, 51.8% aqueous color paste (including 8.5% water, 2.5% dispersant, 0.5% second defoamer, 0.8% second surfactant, 10% inorganic pigment, 0.1% organic pigment, 15% soft filler, 12.1% hard filler, 2% color paste stabilizer and 0.3% neutralizer), 3% first cosolvent, 1% neutralizer, 0.2% thickener and 2% water.

[0173] Component B is composed of the following raw material components in percentage by mass: 75% of curing agent (55% of high viscosity hydrophobic hexamethylene diisocyanate and 20% of hydrophilic modified isophorone diisocyanate) and 25% of the second co-solvent.

[0174] The specific components of the above raw materials are shown in Table 2. After calculation, the solid content of component A is 57.0%.

[0175] The preparation method of the above-mentioned water-based two-component mid-coat paint is the same as that in Example 1 and will not be repeated here.

[0176] Example 5

[0177] This embodiment provides a water-based two-component mid-coat paint, which is composed of component A and component B in a mass ratio of 6:0.7.

[0178] Component A is composed of the following raw material components in percentage by mass: 33% aqueous hydroxyl-containing acrylate dispersion, 3% aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50°C, 3% aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C, 0.6% first surfactant, 0.6% first defoamer, 0.6% substrate wetting agent, 0.6% leveling agent, 49.2% aqueous color paste (including 9% water, 2% dispersant, 0.3% second defoamer, 0.5% second surfactant, 9% inorganic pigment, 0.2% organic pigment, 10.2% soft filler, 15% hard filler, 2.8% color paste stabilizer and 0.2% neutralizer), 4% first cosolvent, 2% neutralizer, 0.4% thickener and 3% water.

[0179] Component B is composed of the following raw material components in percentage by mass: 75% of curing agent (75% of high viscosity hydrophilic hexamethylene diisocyanate) and 25% of the second co-solvent.

[0180] The specific components of the above raw materials are shown in Table 2. After calculation, the solid content of component A is 53.9%.

[0181] The preparation method of the above-mentioned water-based two-component mid-coat paint is the same as that in Example 1 and will not be repeated here.

[0182] Example 6

[0183] This embodiment provides a water-based two-component mid-coat paint, which is composed of component A and component B in a mass ratio of 6:1.7.

[0184] Component A is composed of the following raw material components in percentage by mass: 31% aqueous hydroxyl acrylate dispersion, 4% aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40-50°C, 0.2% first surfactant, 0.2% first defoamer, 0.2% substrate wetting agent, 0.1% leveling agent, 58.1% aqueous color paste (including 12.5% ​​water, 1.6% dispersant, 0.5% second defoamer, 0.8% second surfactant, 9.3% inorganic pigment, 0.3% organic pigment, 15% soft filler, 15% hard filler, 2.8% color paste stabilizer and 0.3% neutralizer), 3% first co-solvent, 1% neutralizer, 0.2% thickener and 2% water.

[0185] Component B is composed of the following raw material components in percentage by mass: 75% of curing agent (75% of hydrophilic modified isophorone diisocyanate) and 25% of the second co-solvent.

[0186] The specific components of the above raw materials are shown in Table 2. After calculation, the solid content of component A is 56.6%.

[0187] The preparation method of the above-mentioned water-based two-component mid-coat paint is the same as that in Example 3 and will not be repeated here.

[0188] Table 2 Specific raw material components of water-based two-component mid-coat paint in Examples 1 to 6

[0189]

[0190]

[0191]

[0192]

[0193] Comparative Example 1

[0194] This comparative example provides a water-based two-component mid-coat paint, which is similar to Example 1, except that Covestro Bayhydrol A2470 is replaced with Covestro Bayhydrol UH 2606 of equal quality (i.e., the water-based resin does not include a water-based hydroxyl-containing acrylate dispersion). The remaining components are the same as those in Example 1 and are not described in detail.

[0195] Comparative Example 2

[0196] This comparative example provides a water-based two-component mid-coat paint, which is similar to Example 1, except that Covestro Bayhydrol UH 2606 is replaced with Covestro Bayhydrol A 2470 of equal quality (i.e., the water-based resin does not contain a water-based polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50° C.). The remaining components are the same as those in Example 1 and are not described in detail.

[0197] Comparative Example 3

[0198] This comparative example provides a water-based two-component mid-coat paint, which is similar to Example 1, except that Covestro Bayhydrol UH 2606 and Bayhydrol UH 2952 / 1 are replaced with Covestro Bayhydrol A2470 of equal quality (i.e., the water-based resin contains only water-based hydroxyl-containing acrylate dispersion). The remaining components are the same as those in Example 1 and are not described in detail.

[0199] Comparative Example 4

[0200] This comparative example provides a water-based two-component mid-coat paint, which is similar to Example 1, except that Covestro Bayhydrol A2470 and Bayhydrol UH 2952 / 1 are replaced by Covestro Bayhydrol UH2606 of equal quality (i.e., the water-based resin contains only a water-based polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50° C.). The remaining components are the same as those in Example 1 and are not described in detail.

[0201] Comparative Example 5

[0202] This comparative example provides a water-based two-component mid-coat paint, which is similar to Example 1, except that Covestro Bayhydrol UH 2606 and Bayhydrol A 2470 are replaced by Covestro Bayhydrol UH2952 / 1 of equal quality (i.e., the water-based resin contains only a water-based polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C). The remaining components are the same as those in Example 1 and are not described in detail.

[0203] Comparative Example 6

[0204] This comparative example provides a water-based two-component mid-coat paint, which is similar to Example 1, except that the water-based resin (Covestro Bayhydrol UH 2606, Bayhydrol A 2470 and Bayhydrol UH 2952 / 1) is replaced with Uacryl 4219 (acrylic emulsion). The remaining components are the same as those in Example 1 and are not described in detail.

[0205] Comparative Example 7

[0206] This comparative example provides a water-based two-component mid-coat paint, which is similar to Example 1, except that Covestro Bayhydrol UH 2606 and Bayhydrol UH 2952 / 1 are replaced by allnex of equal quality. 6803 (water-based acrylic resin emulsion). The remaining components are the same as those in Example 1 and will not be described in detail.

[0207] Application Example 1

[0208] This application embodiment provides a method for using a water-based two-component mid-coat paint, comprising the following steps:

[0209] The components A and B of Example 1 were mixed evenly, and an activated diluent was added and mixed evenly to obtain a construction coating. The mass ratio of the component A to the activated diluent was 100:25.

[0210] The activated diluent is composed of the following raw material components in percentage by mass: 10% aqueous hydroxyl-containing acrylate dispersion, 4% aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50°C, 4% aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C, 29% water-based synthetic sheet silicate solution, 0.6% water-based modified urea solution, 8% first cosolvent, 8% stabilizer, 0.6% defoamer, 0.6% leveling agent and 35.2% water.

[0211] The water-based synthetic sheet silicate solution is composed of the following raw materials in percentage by mass: 2% of organic modified synthetic layer silicate, 2% of emulsifying dispersant and 96% of water.

[0212] It should be noted that the aqueous hydroxyl-containing acrylate dispersion, the aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50° C., the aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5° C., the first cosolvent, the first defoamer and the leveling agent in the activated diluent are the same as the corresponding raw material components in component A of Example 1. The specific components of the remaining raw materials are shown in Table 3.

[0213] Application Example 2

[0214] This application embodiment provides a method for using a water-based two-component mid-coat paint, comprising the following steps:

[0215] The components A and B of Example 2 were mixed evenly, and an activated diluent was added and mixed evenly to obtain a construction coating. The mass ratio of the component A to the activated diluent was 100:20.

[0216] The activated diluent is composed of the following raw material components in percentage by mass: 11.5% aqueous hydroxyl-containing acrylate dispersion, 4.5% aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50°C, 4.5% aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C, 33.5% water-based synthetic sheet silicate solution, 0.7% water-based modified urea solution, 8.4% first cosolvent, 8.5% stabilizer, 0.7% defoamer, 0.7% leveling agent and 27% water.

[0217] The water-based synthetic sheet silicate solution is composed of the following raw materials in percentage by mass: 1.5% of organic modified synthetic layer silicate, 1.5% of emulsifying dispersant and 97% of water.

[0218] It should be noted that the aqueous hydroxyl-containing acrylate dispersion, the aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50° C., the aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5° C., the first cosolvent, the defoamer and the leveling agent in the activated diluent are the same as the corresponding raw material components in component A of Example 2. The specific components of the remaining raw materials are shown in Table 3.

[0219] Application Example 3

[0220] This application embodiment provides a method for using a water-based two-component mid-coat paint, comprising the following steps:

[0221] The components A and B of Example 3 were mixed evenly, and an activated diluent was added and mixed evenly to obtain a construction coating. The mass ratio of the component A to the activated diluent was 100:30.

[0222] The activated diluent is composed of the following raw material components in percentage by mass: 8.1% aqueous hydroxyl-containing acrylate dispersion, 3.1% aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50°C, 3.1% aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C, 27% water-based synthetic sheet silicate solution, 0.5% water-based modified urea solution, 7.6% first cosolvent, 7.6% stabilizer, 0.5% defoamer, 0.5% leveling agent and 42% water.

[0223] The water-based synthetic sheet silicate solution is composed of the following raw materials in percentage by mass: 2.5% of organic modified synthetic layer silicate, 2.5% of emulsifying dispersant and 95% of water.

[0224] It should be noted that the aqueous hydroxyl-containing acrylate dispersion, the aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50° C., the aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5° C., the first cosolvent, the defoamer and the leveling agent in the activated diluent are the same as the corresponding raw material components in component A of Example 3. The specific components of the remaining raw materials are shown in Table 3.

[0225] Application Example 4

[0226] This application embodiment provides a method for using a water-based two-component mid-coat paint, comprising the following steps:

[0227] The components A and B of Example 4 were mixed evenly, and an activated diluent was added and mixed evenly to obtain a construction coating. The mass ratio of the component A to the activated diluent was 100:25.

[0228] The raw material ratio of the activated diluent and the raw material ratio of the water-based synthetic sheet silicate solution are the same as those in Application Example 1; the aqueous hydroxyl-containing acrylate dispersion, the aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50° C., the aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5° C., the first cosolvent, the defoamer and the leveling agent in the activated diluent are the same as the corresponding raw material components in component A of Example 4. The specific components of the remaining raw materials are shown in Table 3.

[0229] Application Example 5

[0230] This application embodiment provides a method for using a water-based two-component mid-coat paint, comprising the following steps:

[0231] The components A and B of Example 5 were mixed evenly, and the activated diluent was added and mixed evenly to obtain a construction coating. The mass ratio of the component A to the activated diluent was 100:25.

[0232] The raw material ratio of the activated diluent and the raw material ratio of the water-based synthetic sheet silicate solution are the same as those in Application Example 1; the aqueous hydroxyl-containing acrylate dispersion, aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50°C, aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C, the first cosolvent, the defoamer and the leveling agent in the activated diluent are the same as the corresponding raw material components in component A of Example 5. The specific components of the remaining raw materials are shown in Table 3.

[0233] Application Example 6

[0234] This application embodiment provides a method for using a water-based two-component mid-coat paint, comprising the following steps:

[0235] The components A and B of Example 6 were mixed evenly, and the activated diluent was added and mixed evenly to obtain a construction coating. The mass ratio of the component A to the activated diluent was 100:25.

[0236] The raw material ratio and components of the activated diluent are the same as those in Application Example 1 and will not be described in detail.

[0237] Table 3 Specific raw material components of the activated diluent in application examples 1 to 5

[0238]

[0239]

[0240] Application Comparative Examples 1 to 7

[0241] Comparative Examples 1 to 7 provide a method for using a water-based two-component mid-coat paint, respectively, comprising the following steps:

[0242] Components A and B of Comparative Examples 1 to 7 were mixed evenly, and activated diluent was added and mixed evenly to obtain 7 groups of construction coatings. The mass ratio of component A to activated diluent was 100:25. The raw material components and proportions of the activated diluent were the same as those of Application Example 1, and will not be described in detail.

[0243] Application Comparative Example 8

[0244] This application comparative example provides a method for using a water-based two-component mid-coat paint, comprising the following steps:

[0245] The components A and B of Example 1 were mixed evenly, and water was added and mixed evenly to obtain a construction coating. The mass ratio of the component A to water was 100:25.

[0246] Application Comparative Example 9

[0247] This comparative application example provides a method for using a water-based two-component mid-coat paint, which is similar to Application Example 1, except that the water-based polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50° C. in the activated diluent is replaced with an equal amount of water-based hydroxyl-containing acrylate dispersion. The remaining conditions are the same as those in Application Example 1 and are not described in detail.

[0248] Application Comparative Example 10

[0249] This comparative application example provides a method for using a water-based two-component mid-coat paint, which is similar to Application Example 1, except that the water-based modified urea solution in the activated diluent is replaced with an equal amount of water-based synthetic sheet silicate solution. The remaining conditions are the same as those in Application Example 1 and are not described in detail.

[0250] Performance Testing

[0251] The performance tests were conducted on the construction coatings provided in Application Examples 1 to 6 and Application Comparative Examples 1 to 10.

[0252] (1) The tinplate was polished with 400-500 mesh sandpaper, and the surface oil was removed with ethanol, and then the construction coatings provided in application examples 1-6 and application comparative examples 1-10 were applied, such as: the construction coatings provided in application examples 1-2, 6 and application comparative examples 1-4 were applied at high temperature and high humidity (38°C, RH=85%), and the construction coatings provided in application examples 3-5 and application comparative examples 5-10 were applied at low temperature and high humidity (0°C, RH=85%); the film thickness was 25μm-35μm, and the coating was baked at 60°C for 2h. The paint film color and appearance, drying time, impact resistance, bending test and cupping test of the obtained test sample were tested respectively, and the test standards are shown in Table 4, and the test results are shown in Tables 5-6.

[0253] (2) On a steel plate coated with a cathode electrophoretic paint (CED, model EcoTa8500, purchased from Shanghai Jinlitai Chemical Co., Ltd.), a WB06-02 primer (purchased from Beijing Yulin Chemical Co., Ltd.) was applied with a film thickness of 60 μm to 70 μm, and baked at 60°C for 2 h; then, the construction coatings provided in Application Examples 1 to 6 and Application Comparative Examples 1 to 10 were applied on the WB06-02 primer, such as: applying the construction coatings provided in Application Examples 3 to 5 and Application Comparative Examples 1 to 4 at high temperature and high humidity (38°C, RH=85%), and applying the construction coatings provided in Application Examples 1 to 2, 6 and Application Comparative Examples 5 to 10 at low temperature and high humidity (0°C, RH=85%); spraying 2 to 3 coats, flashing each coat for 3 min to 5 min, pre-baking at 60°C for 2 h, and after the paint film was cooled to room temperature, applying a WB04-1 topcoat (purchased from Beijing Yulin Chemical Co., Ltd.) with a dry film thickness of 55 μm to 65 μm, and baking at 60°C for 2 h. The solvent wiping resistance, water resistance, gasoline resistance, acid resistance, acid resistance, alkali resistance and artificial climate accelerated aging resistance of the obtained test samples were tested respectively. The test standards are shown in Table 4, and the test results are shown in Tables 5-6.

[0254] Table 4 Performance test standards and requirements of the construction coatings provided in the application examples and comparative examples

[0255]

[0256]

[0257] Note: For any undated referenced standards, the latest version shall apply to this invention.

[0258] Table 5 Performance test results of the construction coating provided by the application example

[0259]

[0260]

[0261] In the table:

[0262] Thixotropic index: measured using NDJ-1 rotary viscometer; viscosity of component A is adjusted by the amount of thickener (ISO6 # ) is about 70s, and its low rotation (6r / min) viscosity and high rotation (60r / min) viscosity are measured. The calculation formula of thixotropic index is: thixotropic index (DI) = low rotation viscosity / high rotation viscosity.

[0263] Appearance effect evaluation: 0 is "excellent", 1 is "qualified", and the larger the number is, the worse it is. 0-smooth and fine; 1-smooth and not fine enough; 2-rough paint film with pinholes; 3-rough paint film with many pits; 4-obvious pinholes and sagging of paint film.

[0264] Construction performance: 0 is "excellent", 1 is "qualified", and the larger the number is, the worse it is. 0-the paint film is smooth and flat, without sagging; 1-slight pitting; 2-slight sagging; 3-pitting and sagging; 4-fly ash, particles, poor fluidity; 5-serious particles, fly ash and serious sagging.

[0265] Cross-cut test: 0 means "excellent", 1 means "qualified", and the larger the number is, the worse it is. 0-The substrate is not polished, and the adhesion is excellent; the rest is based on the cross-cut test standard GB / T9286-1998 "Cross-cut test for paint and varnish film".

[0266] Table 6 Performance test results of the construction coating provided by the comparative example

[0267]

[0268]

[0269]

[0270] In summary, the water-based two-component mid-coat provided by the present invention, component A uses a water-based hydroxyl-containing acrylate dispersion and a water-based polycarbonate-containing aliphatic anionic polyurethane dispersion with a high glass transition temperature to compound as a film-forming resin, and a water-based aliphatic anionic polyurethane dispersion with a low glass transition temperature is selectively added. Through a specific ratio and the synergistic effect of each component, the characteristics of different types of water-based resins are brought into an optimal state, so that the final water-based two-component mid-coat has good thixotropy, and the paint film has excellent characteristics such as high gloss, high fullness and small orange peel. Moreover, when spraying on a large area, no fly ash is produced, the gun is well mounted, and the thixotropy is improved. At the same time, the flexibility and hardness of the cured film are balanced, and large-scale construction can be carried out under high temperature, low temperature or high humidity environments. Through the synergistic effect of various raw material components and specific proportion content, the primer does not need to be polished, and the water-based two-component mid-coat of the present invention can be directly sprayed. After the coating is completed and dried, the topcoat can be sprayed without polishing. The paint film is flat and smooth, and the appearance gloss (60°) is 60-80, which is convenient for checking the paint film for pinholes, flatness, etc., improves the inspection efficiency, ensures the inspection accuracy, thereby reducing the accident risk of rail transit vehicles, and has high practical value and promotion value.

[0271] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A water-based two-component mid-coat paint, characterized in that: It is composed of component A and component B in a mass ratio of 6:0.6 to 6:1.9; wherein, The component A comprises the following raw material components in percentage by mass: 30% to 35% of aqueous hydroxyl-containing acrylate dispersion, 3% to 10% of aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50°C, 0 to 10% of aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C, 0.2% to 1% of a first surfactant, 0.2% to 1% of a first defoamer, 0.2% to 1% of a substrate wetting agent, 0.1% to 1% of a leveling agent, 40% to 60% of an aqueous color paste, 3% to 6% of a first cosolvent, 1% to 3% of a neutralizer, 0.2% to 0.6% of a thickener, and 2% to 5% of water; The hydroxyl content of the aqueous hydroxyl-containing acrylate dispersion is 3.5% to 4.5%, and the solid content of the aqueous hydroxyl-containing acrylate dispersion is 40% to 50%; the aqueous color paste comprises water, a dispersant, a second defoamer, a second surfactant, a pigment, a filler, a color paste stabilizer and a neutralizer; The B component includes the following raw material components in percentage by mass: 70% to 80% of a curing agent and 20% to 30% of a second co-solvent; the curing agent is at least one of hexamethylene diisocyanate or a hydrophilic aliphatic polyisocyanate.

2. The water-based two-component mid-coat paint according to claim 1, characterized in that: The viscosity of the aqueous hydroxyl-containing acrylate dispersion is 1000 mPa·s to 3000 mPa·s; The solid contents of the aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50° C. and the aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5° C. are both 33% to 42%.

3. The water-based two-component mid-coat paint according to claim 1, characterized in that: The aqueous hydroxyl-containing acrylate dispersion is at least one of Covestro Bayhydrol A 2470, Covestro Bayhydrol A 2770 or Covestro Bayhydrol A 2601; The aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion having a glass transition temperature of 40 to 50° C. is Bayhydrol UH 2606 from Covestro; The aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5° C. is at least one of Bayhydrol UH2648 / 1, Bayhydrol UH 2110, Bayhydrol UH 2621 or Bayhydrol UH2952 / 1.

4. The water-based two-component mid-coat paint according to claim 1, characterized in that: Taking the A component as 100%, the water-based color paste includes 8.5% to 12.5% ​​of water, 1.5% to 2.5% of dispersant, 0.2% to 0.5% of second defoamer, 0.2% to 0.8% of second surfactant, 8% to 10% of inorganic pigment, 0.1% to 0.3% of organic pigment, 10% to 15% of soft filler, 10% to 15% of hard filler, 1.4% to 2.8% of color paste stabilizer and 0.1% to 0.3% of neutralizer; The fineness of the water-based color paste is 20 μm to 30 μm.

5. The water-based two-component mid-coat paint according to claim 1, characterized in that: Taking the B component as 100%, the curing agent comprises 25% to 30% of low-viscosity hydrophobic hexamethylene diisocyanate, 25% to 30% of high-viscosity hydrophilic hexamethylene diisocyanate and 18% to 22% of hydrophilic modified isophorone diisocyanate; wherein, The solid content of the hydrophilic aliphatic polyisocyanate is 60% to 70%, and the -NCO content of the hydrophilic aliphatic polyisocyanate is 8.5% to 12%.

6. The water-based two-component mid-coat paint according to claim 5, characterized in that: The low-viscosity hydrophobic hexamethylene diisocyanate is at least one of Covestro Desmodur N3900, Covestro Desmodur N3600 or Wanhua WANNATE HT-600; The high-viscosity hydrophilic hexamethylene diisocyanate is at least one of Covestro Bayhydrol XP 2655, Covestro Bayhydur XP 2547, Covestro Bayhydur XP 2487 / 1, Covestro Bayhydur 304 or Covestro Bayhydur 305; The hydrophilic aliphatic polyisocyanate is at least one of Covestro Bayhydur 401-70 and Covestro Bayhydur 401-60.

7. The water-based two-component mid-coat paint according to any one of claims 1 to 6, characterized in that: The first cosolvent comprises at least three of propylene glycol methyl ether propionate, propylene glycol butyl ether, dipropylene glycol dimethyl ether, ethylene glycol butyl ether, dipropylene glycol methyl ether, dimethyl sulfoxide, N-methylpyrrolidone, dipropylene glycol butyl ether or diethylene glycol monobutyl ether; The second cosolvent is at least two of propylene glycol methyl ether acetate, propylene glycol methyl ether acrylate, propylene glycol diacetate, ethylene glycol butyl ether acetate, dipropylene glycol dimethyl ether, propylene carbonate or dibasic acid ester; The dispersant is at least one of a nonionic wetting dispersant or an anionic wetting dispersant; The second surfactant is at least one of an acetylenic glycol surfactant or an alcohol alkoxy compound; The color paste stabilizer includes at least three of water-based fumed silica, organically modified montmorillonite clay rheological additives, modified urea rheological additives, resin-free color paste moisturizers, or anti-drying agents for water-based pigment concentrates; The neutralizing agent is an aqueous solution of 8wt% to 12wt% dimethylethanolamine; The first surfactant is a gemini acetylenic diol surfactant; The substrate wetting agent is a polyether-modified silicone surfactant; The thickener is a polyurethane associative thickener.

8. Use of the water-based two-component mid-coat paint according to any one of claims 1 to 7 in automotive coatings.

9. The method for using the water-based two-component mid-coat paint according to any one of claims 1 to 7, characterized in that: The following steps are involved: Mix component A and component B evenly, add an activated diluent, mix evenly to obtain a construction coating, and evenly apply it on the water-based base paint; The activated diluent comprises an aqueous hydroxyl-containing acrylate dispersion, an aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50° C., an aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5° C., a water-based synthetic sheet silicate solution, a water-based modified urea solution, a first cosolvent, a stabilizer, a first defoamer, a leveling agent and water.

10. The method for using the water-based two-component mid-coat paint according to claim 9, characterized in that: The activated diluent comprises the following raw material components in mass percentage: 8% to 11.5% of aqueous hydroxyl-containing acrylate dispersion, 3% to 4.5% of aqueous polycarbonate-containing aliphatic anionic polyurethane dispersion with a glass transition temperature of 40 to 50°C, 3% to 4.5% of aqueous aliphatic anionic polyurethane dispersion with a glass transition temperature of ≤5°C, 25% to 33.5% of water-based synthetic sheet silicate solution, 0.5% to 0.7% of water-based modified urea solution, 7.5% to 8.5% of a first cosolvent, 7.5% to 8.5% of a stabilizer, 0.5% to 0.7% of a first defoamer, 0.5% to 0.7% of a leveling agent, and 27% to 42% of water, the sum of the components being 100%; The mass ratio of the A component to the activated diluent is 100:(20-30); The water-based synthetic sheet silicate solution comprises the following raw material components in mass percentage: 1.5% to 2.5% of organic modified synthetic sheet silicate, 1.5% to 2.5% of emulsifying dispersant and 95% to 97% of water, the sum of the components being 100%; The water-based modified urea solution is at least one of BYK RHEOBYK-7420CA, BYK RHEOBYK-7420ET or BYK RHEOBYK-7420ES.

Citation Information

Patent Citations

  • Aqueous primer surfacer

    CN102250541A

  • A waterborne automobile coating composition and a preparing method and applications thereof

    CN107099238A

  • Two-component waterborne polyurethane coating composition with thixotropic flow characteristic, and preparation method thereof

    CN109535973A

  • Preparation method of water-based two-component intermediate coating composition for special vehicle

    CN115678402A

  • High-solid-content three-coating and one-baking intermediate coat for automobile based on water-based acrylic resin and application of intermediate coat

    CN116925610A