Composite solvent cerium-based polishing solution and preparation method thereof

By using organic solvents and deionized water in the polishing liquid to form a composite solvent system, combined with high-speed shearing and ultrasonic treatment, the problem of poor abrasive particles is solved, and the high suspension and dispersion of the polishing liquid is achieved, which significantly improves the Polishing effect and sample surface quality.

CN118978864APending Publication Date: 2024-11-19XIAN RARE METAL MATERIALS RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411046780.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The poor morphology of the abrasive particles in the existing polishing liquid leads to high surface roughness of the sample after polishing, and the existing dispersion method has a large strength, which will cause the surface morphology of the abrasive particles to be damaged, affecting the polishing effect.

Method used

The organic solvent and deionized water are used to form a composite solvent system, and the dispersant and consolidation preventing agent are added. The CeO2 abrasive particles are evenly dispersed through high-speed shearing and ultrasonic treatment. The pH adjuster and oxidizing agent are combined to form a medium/alkaline cerium-based polishing. to maintain the morphology of the abrasive particles and improve suspension and dispersion.

Benefits of technology

The uniform dispersion and stability of CeO2 abrasive particles are achieved, the suspension and dispersion of the polishing liquid are improved, the surface quality and piercing rate of the sample after polishing are significantly improved, and the surface damage of the abrasive particles is avoided.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978864A_ABST
    Figure CN118978864A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a composite solvent cerium-based polishing solution, which comprises the following steps: step 1, mixing an organic solvent with deionized water to form a composite solvent, adding a dispersing agent and a consolidation preventing agent, and uniformly mixing; 2, adding CeO2 abrasive particles, sequentially carrying out high-speed shearing and ultrasonic treatment, and standing; 3, adding a pH regulator to adjust the pH value to 7-10, then adding an oxidizing agent to carry out ultrasonic dispersion, and uniformly mixing to obtain a cerium-based polishing solution; the invention further discloses the composite solvent cerium-based polishing solution. According to the preparation method, an organic solvent and deionized water are introduced to form a composite solvent system, CeO2 abrasive particles are uniformly dispersed after being subjected to high-speed shearing and ultrasonic treatment, then the pH value is regulated by adopting a pH regulator, and the neutral and alkaline cerium-based polishing solution which is intact in CeO2 abrasive particle surface appearance and excellent in suspension property and dispersity is obtained and is suitable for being applied to the technical field of polishing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polishing, and in particular relates to a composite solvent cerium-based polishing liquid and a preparation method thereof. Background Art

[0002] Chemical mechanical polishing (CMP) is an industrial processing technology that can achieve high-precision flattening. It is widely used in semiconductors, optical glass, ceramic substrates and other fields. The CMP system is mainly composed of polishing equipment, polishing pads, and polishing liquid. During operation, the wafer and the polishing pad move relative to each other under a certain load and polishing liquid, and the flattening polishing of the substrate surface is achieved through chemical and mechanical effects to achieve low surface roughness, low defects and other requirements. Polishing liquid is an important factor affecting CMP performance. It is generally composed of abrasives, additives and solvents to achieve surface softening, corrosion and grinding during the processing process. The abrasives are generally micron or submicron solid particles with a certain hardness, including CeO2, SiO2, diamond, Al2O3, etc., which can be used for different needs.

[0003] Cerium-based polishing liquid uses cerium-based compounds such as CeO2 and LnOF as abrasive particles, which can achieve good mechanical processing effects on wafers, optical glass, etc., and has a good application basis. The abrasive particles evenly dispersed in the polishing liquid can effectively improve the surface quality, and the synergistic effect of components such as oxidants and pH regulators can accelerate the chemical corrosion during the polishing process and improve processing efficiency.

[0004] At present, researchers have conducted a variety of studies on polishing liquids. According to the pH value, polishing liquids can be divided into acidic and alkaline polishing liquids. CeO2 in acidic polishing liquids will undergo acid hydrolysis after long-term storage, and has higher requirements for the anti-corrosion performance of equipment during application. Alkaline polishing liquids have lower requirements for equipment during application, higher stability, and a wider range of applications. However, in the prior art, abrasive processing usually adopts ball milling or dispersion disk dispersion. These two dispersion methods have high processing intensity and will wear the surface morphology of abrasive particles, resulting in poor abrasive morphology in the polishing liquid and poor surface roughness of the sample after polishing. Summary of the invention

[0005] The purpose of the present invention is to overcome the deficiencies in the above-mentioned prior art and provide a method for preparing a composite solvent cerium-based polishing liquid. The preparation method introduces an organic solvent and deionized water to form a composite solvent system, then adds a dispersant and a solidification inhibitor, so that CeO2 abrasive particles are uniformly dispersed in the composite solvent after high-speed shearing and ultrasonic treatment, and then uses a pH regulator to adjust the pH value to obtain a medium / alkaline cerium-based polishing liquid with intact CeO2 abrasive surface morphology and excellent suspension and dispersibility, thereby solving the problem in the prior art that the poor morphology of the abrasive particles in the polishing liquid affects the surface roughness of the sample after polishing.

[0006] To achieve the above object, the technical solution adopted by the present invention is: a method for preparing a composite solvent cerium-based polishing liquid, characterized in that the method comprises the following steps:

[0007] Step 1: Mixing an organic solvent with deionized water to form a composite solvent, and then uniformly mixing a dispersant and an anti-solidification agent with the composite solvent to obtain a solution A;

[0008] Step 2, adding CeO2 abrasive to the solution A obtained in step 1, performing high-speed shearing and ultrasonic treatment in sequence, and then standing to form a slurry;

[0009] Step 3: Add a pH adjuster to the slurry formed in step 2 to adjust the pH value to 7-10, add an oxidant to perform ultrasonic dispersion, and obtain a cerium-based polishing liquid.

[0010] The invention introduces an organic solvent to cooperate with a dispersant to assist the dispersion of abrasive particles, thereby improving the suspension and dispersibility of abrasive particles in the polishing liquid.

[0011] The present invention disperses CeO2 abrasive particles by adopting high-speed shearing and ultrasonic treatment. High-speed shearing is a high-speed stirring of a high-speed airflow in a liquid phase, which preliminarily breaks up the soft agglomerates between the abrasive particles. Ultrasonic treatment is then used to further disperse the abrasive particles so as to dissolve the agglomerates, and finally the CeO2 abrasive particles are dispersed and have a uniform particle size distribution. Meanwhile, the CeO2 abrasive particles are not ground during the high-speed shearing and ultrasonic treatment process, and the particle morphology of the abrasive particles can be kept intact.

[0012] The method for preparing the composite solvent cerium-based polishing liquid is characterized in that the mass of the organic solvent in step 1 accounts for 0.1% to 50% of the total mass of the composite solvent, and the organic solvent is a water-soluble organic solvent.

[0013] The method for preparing the composite solvent cerium-based polishing liquid is characterized in that the water-soluble organic solvent is one or more of methanol, ethanol, glycerol, ethylene glycol and n-butanol.

[0014] The method for preparing the composite solvent cerium-based polishing liquid is characterized in that the mass of the dispersant in step 1 accounts for 0.001% to 10% of the total mass of the composite solvent, and the dispersant is a surfactant without metal cations.

[0015] The present invention avoids the introduction of Na into the polishing liquid by selecting a surfactant without metal cations. + , K + Metal cations such as fluorine have adverse effects on the structure and properties of polished samples during wafer polishing and optical glass processing; surfactants include polyvinyl pyrrolidone, polyethylene glycol, acetylacetone, OP-10, EDTA, carboxymethyl cellulose and hydroxyethyl cellulose.

[0016] The above-mentioned method for preparing a composite solvent cerium-based polishing liquid is characterized in that the mass of the anti-solidification agent in step one accounts for 0.001% to 5% of the total mass of the composite solvent, and the anti-solidification agent is one or more of silicic acid, silicone gel, acetic acid, citric acid and glacial acetic acid.

[0017] The present invention selects compounds with a certain network structure in the solution, such as silicic acid, silica gel, acetic acid, citric acid and glacial acetic acid, to form a separation layer on the surface of the abrasive particles so that the precipitated abrasive particles will not be agglomerated and can be easily redispersed. At the same time, the selected anti-agglomeration agent will not introduce Na + , K + etc. metal cations.

[0018] The method for preparing the composite solvent cerium-based polishing liquid is characterized in that the mass of the CeO2 abrasive particles in step 2 accounts for 0.1% to 30% of the total mass of the slurry.

[0019] The above-mentioned method for preparing a composite solvent cerium-based polishing liquid is characterized in that the high-speed shearing time in step 2 is 30min to 60min, the high-speed shearing speed is 6000r / min to 12000r / min, the ultrasonic treatment time is 20min to 90min, and the standing time is 1h to 24h.

[0020] The present invention can evenly disperse CeO2 abrasive particles by setting the high-speed shearing time at 30 min to 60 min. When the high-speed shearing time is less than 30 min, the CeO2 abrasive particles are unevenly stirred and dispersed, and sediments quickly accumulate at the bottom of the container after the high-speed shearing ends. When the high-speed shearing time is more than 60 min, the CeO2 abrasive particles will collide violently and agglomerate, resulting in secondary agglomeration. The dispersion requirements can be met by setting the ultrasonic treatment time at 20 min to 90 min. When the ultrasonic treatment time is less than 20 min, the dispersion effect is poor, and when the time is more than 90 min, the dispersion degree of the CeO2 abrasive particles remains basically unchanged.

[0021] The method for preparing the composite solvent cerium-based polishing liquid is characterized in that the particle size D50 of the CeO2 abrasive particles in the slurry in step 2 is 400nm to 600nm.

[0022] The invention uses high-speed shearing and ultrasonic treatment to make the particle size D50 of CeO2 abrasive particles be 400nm-600nm. The particle size distribution range can improve the polishing rate of the polishing liquid and the surface quality of the sample after polishing.

[0023] The method for preparing the composite solvent cerium-based polishing liquid is characterized in that the pH regulator in step three is ammonia water and the oxidant is hydrogen peroxide.

[0024] The present invention can soften the surface of the polishing sample by utilizing the oxidation effect of hydrogen peroxide, thereby improving the polishing efficiency.

[0025] The invention also discloses a composite solvent cerium-based polishing liquid, which is characterized in that it is prepared by the preparation method of the composite solvent cerium-based polishing liquid.

[0026] Compared with the prior art, the present invention has the following advantages:

[0027] 1. The present invention introduces an organic solvent and deionized water to form a composite solvent system, so that the composite solvent and the dispersant act together on CeO2 abrasive particles to improve the dispersion effect, and further evenly disperses the CeO2 abrasive particles through high-speed shearing and ultrasonic treatment, so that the obtained cerium-based polishing liquid has excellent suspension, dispersibility and stability; at the same time, the CeO2 abrasive particles are dispersed through high-speed shearing and ultrasonic treatment, which avoids the problem in the prior art that the CeO2 abrasive particles are unable to maintain the morphology of the CeO2 abrasive particles intact by using ball milling or dispersion disk dispersion.

[0028] 2. The present invention adopts a water-soluble organic solvent to reduce the viscosity of the finished polishing liquid, so that the cleaning of the sample after polishing is simpler and faster.

[0029] 3. The present invention adopts the method of not introducing Na + , K + Organic solvents, dispersants and anti-solidification agents for metal cations such as Na + , K + Metal cations such as ions have adverse effects on the structure and properties of polished samples during wafer and optical glass processing.

[0030] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is the initial microscopic morphology of the CeO2 abrasive in Example 1.

[0032] Figure 2 This is a microscopic morphology of CeO2 abrasive particles in the cerium-based polishing liquid in Example 1.

[0033] Figure 3 This is the particle size distribution diagram of CeO2 abrasive in the slurry in Example 1.

[0034] Figure 4 These are photos of the polishing solutions of Comparative Example 1 and Example 2 after standing for 1 hour.

[0035] Figure 5 These are photos of the polishing solutions of Comparative Example 1 and Example 2 after being left to stand for 1 day.

[0036] Figure 6These are photos of the polishing solutions of Comparative Example 1 and Example 2 after standing for 7 days. DETAILED DESCRIPTION

[0037] Example 1

[0038] The preparation method of this embodiment comprises the following steps:

[0039] Step 1: 5 mL of ethanol, 2 mL of ethylene glycol and 2 mL of glycerol were mixed with 88 mL of deionized water to form a composite solvent, and then 1 g of polyvinyl pyrrolidone, 0.5 g of polyethylene glycol and 0.5 mL of glacial acetic acid were added and mixed evenly with the composite solvent to obtain solution A;

[0040] Step 2: Add 15 g of CeO2 abrasive to the solution A obtained in step 1, perform high-speed shearing for 40 min and ultrasonic treatment for 60 min, and then stand for 10 h to form a slurry; the high-speed shearing speed is 12000 r / min;

[0041] Step 3: Add ammonia water to the slurry formed in step 2 to adjust the pH value to 7, add 3 mL of hydrogen peroxide to perform ultrasonic dispersion, and then mix well to obtain a cerium-based polishing liquid.

[0042] The ethanol, ethylene glycol and glycerol described in this embodiment can also be replaced by one or two of methanol and n-butanol other than ethanol, ethylene glycol and glycerol, and the glacial acetic acid can also be replaced by one or more of silicic acid, silicone gel, acetic acid and citric acid other than glacial acetic acid.

[0043] The initial microscopic morphology of CeO2 abrasive particles and the microscopic morphology of CeO2 abrasive particles in the cerium-based polishing liquid in this embodiment were photographed using a scanning electron microscope. Figure 1 and Figure 2 As shown in the figure, the microstructure of CeO2 abrasive particles did not change significantly, and the particle morphology was intact.

[0044] The particle size of CeO2 abrasive particles in the slurry obtained in step 2 of this embodiment was detected. Figure 3 As shown, the particle size distribution of CeO2 abrasive particles is mainly concentrated in the range of 0 μm to 1 μm, with a particle size D50 of 404 nm. This particle size can improve the polishing rate and surface quality of the polishing liquid.

[0045] Example 2

[0046] The preparation method of this embodiment comprises the following steps:

[0047] Step 1: 10 mL of ethanol, 10 mL of ethylene glycol and 10 mL of glycerol were mixed with 67 mL of deionized water to form a composite solvent, and then 3 g of polyethylene glycol, 1.8 g of acetylacetone and 1.5 g of citric acid were added and mixed evenly with the composite solvent to obtain solution A;

[0048] Step 2: Add 20 g of CeO2 abrasive to the solution A obtained in step 1, perform high-speed shearing for 30 min and ultrasonic treatment for 30 min in sequence, and then stand for 16 h to form a slurry; the particle size D50 of the CeO2 abrasive in the slurry is 593 nm; the high-speed shearing speed is 6000 r / min;

[0049] Step 3: Add ammonia water to the slurry formed in step 2 to adjust the pH value to 8, add 3 mL of hydrogen peroxide to perform ultrasonic dispersion, and then mix well to obtain a cerium-based polishing liquid.

[0050] Comparative Example 1

[0051] The difference between this comparative example and Example 2 is that: Step 3 is to add hydrochloric acid to the slurry formed in Step 2 to adjust the pH value to 4, add 3 mL of hydrogen peroxide to perform ultrasonic dispersion, and then mix evenly to obtain a polishing liquid.

[0052] The polishing liquids prepared in this comparative example and Example 2 were allowed to stand for 1 h, 1 d and 7 d respectively. Figures 4 to 6 As shown, polishing liquid No. 1 is the polishing liquid prepared in this comparative example, and polishing liquid No. 2 is the polishing liquid prepared in Example 2; after standing for 1 hour, polishing liquid No. 1 has a supernatant liquid and produces obvious stratification; after standing for 1 day, the abrasive particles in polishing liquid No. 1 completely settle and gather at the bottom of the beaker, and the abrasive particles in polishing liquid No. 2 begin to settle; after standing for 7 days, polishing liquid No. 2 has a supernatant liquid and produces obvious stratification, but the precipitate can be easily dispersed after stirring; since hydrochloric acid is used to adjust the pH value to 4, the polishing liquid prepared in this comparative example is more prone to sedimentation and particle agglomeration than the polishing liquid prepared in Example 2, and has poor stability.

[0053] Example 3

[0054] The preparation method of this embodiment comprises the following steps:

[0055] Step 1: 10 mL of methanol and 10 mL of ethylene glycol were mixed with 77 mL of deionized water to form a composite solvent, and then 2 mL of OP-10, 4 g of polyethylene glycol and 2 g of silicic acid were added and mixed evenly with the composite solvent to obtain solution A;

[0056] Step 2: Add 20 g of CeO2 abrasive to the solution A obtained in step 1, perform high-speed shearing for 60 min and ultrasonic treatment for 60 min in sequence, and then stand for 24 h to form a slurry; the particle size D50 of the CeO2 abrasive in the slurry is 470 nm; the high-speed shearing speed is 10000 r / min;

[0057] Step 3: Add ammonia water to the slurry formed in step 2 to adjust the pH value to 7, add 3 mL of hydrogen peroxide to perform ultrasonic dispersion, and then mix well to obtain a cerium-based polishing liquid.

[0058] Example 4

[0059] The preparation method of this embodiment comprises the following steps:

[0060] Step 1: 30 mL of ethanol and 67 mL of deionized water were mixed to form a composite solvent, and then 1 g of polyvinyl pyrrolidone, 1.5 g of polyethylene glycol and 2.5 g of silicic acid were added and mixed evenly with the composite solvent to obtain solution A;

[0061] Step 2: Add 10 g of CeO2 abrasive to the solution A obtained in step 1, perform high-speed shearing for 40 min and ultrasonic treatment for 60 min, and then stand for 16 h to form a slurry; the particle size D50 of the CeO2 abrasive in the slurry is 502 nm; the high-speed shearing speed is 8000 r / min;

[0062] Step 3: Add ammonia water to the slurry formed in step 2 to adjust the pH value to 9, add 3 mL of hydrogen peroxide to perform ultrasonic dispersion, and then mix well to obtain a cerium-based polishing liquid.

[0063] Example 5

[0064] The preparation method of this embodiment comprises the following steps:

[0065] Step 1: 7 mL of methanol, 7 mL of ethanol, 6 mL of ethylene glycol and 77 mL of deionized water were mixed to form a composite solvent, and then 0.1 g of EDTA, 1.5 g of acetylacetone and 1.5 g of citric acid were added and mixed evenly with the composite solvent to obtain solution A;

[0066] Step 2: Add 10 g of CeO2 abrasive to the solution A obtained in step 1, perform high-speed shearing for 30 min and ultrasonic treatment for 30 min in sequence, and then stand for 16 h to form a slurry; the particle size D50 of the CeO2 abrasive in the slurry is 565 nm; the high-speed shearing speed is 6000 r / min;

[0067] Step 3: Add ammonia water to the slurry formed in step 2 to adjust the pH value to 8, add 3 mL of hydrogen peroxide to perform ultrasonic dispersion, and then mix well to obtain a cerium-based polishing liquid.

[0068] Comparative Example 2

[0069] The difference between this comparative example and Example 5 is that in step 1, only 97 mL of deionized water is used as the solvent, and no organic solvents such as methanol, ethanol and ethylene glycol are added; and 2 g of CeO2 abrasive is added in step 2.

[0070] Compared with Example 5, the concentration of dispersible abrasive in the polishing liquid prepared in this comparative example is greatly reduced, affecting the polishing rate of the polishing liquid; during the preparation process of this comparative example, when the mass of CeO2 abrasive added in step 2 is greater than 4g, high-speed shearing and ultrasonic treatment are performed in sequence and then allowed to stand, the formed slurry immediately stratifies and produces a large amount of precipitation, and cannot form a suspension; this shows that the composite solvent system formed by the organic solvent and deionized water can work together with the dispersant to improve the dispersion effect of the CeO2 abrasive.

[0071] Example 6

[0072] The preparation method of this embodiment comprises the following steps:

[0073] Step 1: 15 mL of ethanol and 85 mL of deionized water were mixed to form a composite solvent, and then 4 g of polyvinyl pyrrolidone, 0.5 g of carboxymethyl cellulose and 0.5 g of citric acid were added and mixed evenly with the composite solvent to obtain solution A;

[0074] Step 2: Add 10 g of CeO2 abrasive to the solution A obtained in step 1, perform high-speed shearing for 30 min and ultrasonic treatment for 90 min, and then stand for 1 h to form a slurry; the particle size D50 of the CeO2 abrasive in the slurry is 540 nm; the high-speed shearing speed is 6000 r / min;

[0075] Step 3: Add ammonia water to the slurry formed in step 2 to adjust the pH value to 10, add 3 mL of hydrogen peroxide to perform ultrasonic dispersion, and then mix well to obtain a cerium-based polishing liquid.

[0076] Example 7

[0077] The preparation method of this embodiment comprises the following steps:

[0078] Step 1: 2 mL of ethylene glycol and 98 mL of deionized water were mixed to form a composite solvent, and then 1 g of polyvinyl pyrrolidone, 4 g of polyethylene glycol and 5 g of silicic acid were added and mixed evenly with the composite solvent to obtain solution A;

[0079] Step 2: Add 10 g of CeO2 abrasive to the solution A obtained in step 1, perform high-speed shearing for 60 min and ultrasonic treatment for 20 min, and then stand for 16 h to form a slurry; the particle size D50 of the CeO2 abrasive is 550 nm; the high-speed shearing speed is 12000 r / min;

[0080] Step 3: Add ammonia water to the slurry formed in step 2 to adjust the pH value to 9, add 3 mL of hydrogen peroxide to perform ultrasonic dispersion, and then mix well to obtain a cerium-based polishing liquid.

[0081] Example 8

[0082] The preparation method of this embodiment comprises the following steps:

[0083] Step 1: Mix 10 mL of ethanol and 87 mL of deionized water and stir evenly, then add 3 g of polyvinyl pyrrolidone, 3 g of polyethylene glycol, 2 g of hydroxyethyl cellulose, 2 g of OP-10 and 2.5 g of silicic acid and mix evenly to obtain solution A;

[0084] Step 2: Add 30 g of CeO2 abrasive to the solution A obtained in step 1, mix thoroughly, and perform high-speed shearing for 60 min and ultrasonic treatment for 60 min in sequence, so that the CeO2 abrasive is fully dispersed and then soaked and allowed to stand for 16 h to form a slurry; the particle size D50 of the CeO2 abrasive in the slurry is 532 nm; the high-speed shearing speed is 10000 r / min;

[0085] Step 3: Add ammonia water to the slurry formed in step 2 to adjust the pH value to 9, add 3 mL of hydrogen peroxide to perform ultrasonic dispersion, and then mix well to obtain a cerium-based polishing liquid.

[0086] Comparative Example 3

[0087] The preparation process of the polishing liquid of this comparative example is as follows: hydrochloric acid is added to deionized water to prepare 100 mL of an acidic solution with a pH value of 4, 4 g of CeO2 abrasive is added, high-speed shearing is performed for 30 minutes, ultrasonic treatment is performed for 30 minutes in sequence to make a slurry, and the polishing liquid is obtained after standing for 5 hours.

[0088] Comparative Example 4

[0089] The preparation process of the polishing liquid of this comparative example is:

[0090] Step 1: Add 10 g of CeO2 abrasive to 30 mL of deionized water and ball mill for 2 h to obtain CeO2 abrasive slurry; the ball mill uses agate balls, the ball-to-material ratio is 10:1, and the rotation speed is 300 r / min;

[0091] Step 2: Add 3 g of polyvinyl pyrrolidone, 3 g of polyethylene glycol and 2 g of citric acid to 67 mL of deionized water to obtain solution B;

[0092] Step 3: Mix the CeO2 abrasive slurry obtained in step 1 with solution B obtained in step 2, add ammonia water to adjust the pH to 9, add 3 mL of hydrogen peroxide, ultrasonically treat for 30 minutes, and then soak and stand for 5 hours to obtain a polishing solution.

[0093] The polishing liquids prepared in Examples 1 to 8, Comparative Example 1 and Comparative Examples 3 to 4 were diluted to a CeO2 abrasive mass concentration of 1%, and polishing tests were performed. The polishing tests were performed using a Shenyang Kejing UNIPOL-1200S single-sided polishing machine and a polyurethane polishing pad. The polishing liquid flow rate was set to 25 mL / min, the polishing conditions were a pressure of 3.5 kg, a polishing time of 10 min, an upper polishing disc speed of 80 rpm / min, a lower polishing disc speed of 80 rpm / min, and the polishing sample was a Ф30 mm H-K9 optical glass.

[0094] After polishing, all polished glass sheets were ultrasonically cleaned and dried under the same conditions, and the polishing rate and surface roughness of the polished samples were tested.

[0095] Table 1 Polishing liquid performance test values ​​of Examples 1 to 8, Comparative Example 1 and Comparative Examples 3 to 4

[0096] Cutting rate (nm / min) Surface roughness(nm) Example 1 545 0.67 Example 2 602 0.56 Example 3 664 0.49 Example 4 466 0.52 Example 5 620 0.61 Example 6 561 0.54 Example 7 543 0.60 Example 8 588 0.51 Comparative Example 1 245 Obvious surface defects Comparative Example 3 356 0.4 Comparative Example 4 375 0.55

[0097] It can be seen from Table 1 that the polishing rate of the composite solvent cerium-based polishing liquid prepared in Examples 1 to 8 is not less than 466nm / min, and the roughness of the sample surface after polishing is not greater than 0.67nm. Under the condition that the mass concentration of CeO2 abrasive is 1%, the polishing rates of the polishing liquids of Comparative Example 1, Comparative Example 3 and Comparative Example 4 are significantly reduced compared with the medium / alkaline polishing liquids prepared in Examples 1 to 8; among them, Comparative Example 1 and Comparative Example 3 are acidic polishing liquids with poor polishing performance, and the polishing liquid of Comparative Example 4 is ball-milled without adding a composite solvent system, which destroys the integrity of the abrasive and causes its polishing rate to decrease.

[0098] In summary, the polishing liquids prepared in Examples 1 to 8 of the present invention have the characteristics of high polishing rate and good polishing effect.

[0099] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent structural transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing a composite solvent cerium-based polishing liquid, characterized in that: The preparation method comprises the following steps: Step 1: Mixing an organic solvent with deionized water to form a composite solvent, and then uniformly mixing a dispersant and an anti-solidification agent with the composite solvent to obtain a solution A; Step 2, adding CeO2 abrasive to the solution A obtained in step 1, performing high-speed shearing and ultrasonic treatment in sequence, and then standing to form a slurry; Step 3: Add a pH adjuster to the slurry formed in step 2 to adjust the pH value to 7-10, add an oxidant to perform ultrasonic dispersion, and obtain a cerium-based polishing liquid.

2. The method for preparing a composite solvent cerium-based polishing liquid according to claim 1, characterized in that: The mass of the organic solvent in step 1 accounts for 0.1% to 50% of the total mass of the composite solvent, and the organic solvent is a water-soluble organic solvent.

3. The method for preparing a composite solvent cerium-based polishing liquid according to claim 2, characterized in that: The water-soluble organic solvent is one or more of methanol, ethanol, propylene glycol, ethylene glycol and n-butanol.

4. The method for preparing a composite solvent cerium-based polishing liquid according to claim 1, characterized in that: The mass of the dispersant in step 1 accounts for 0.001% to 10% of the total mass of the composite solvent, and the dispersant is a surfactant without metal cations.

5. The method for preparing a composite solvent cerium-based polishing liquid according to claim 1, characterized in that: The mass of the anti-solidification agent in step 1 accounts for 0.001% to 5% of the total mass of the composite solvent, and the anti-solidification agent is one or more of silicic acid, silica gel, acetic acid, citric acid and glacial acetic acid.

6. The method for preparing a composite solvent cerium-based polishing liquid according to claim 1, characterized in that: In step 2, the mass of the CeO2 abrasive particles accounts for 0.1% to 30% of the total mass of the slurry.

7. The method for preparing a composite solvent cerium-based polishing liquid according to claim 1, characterized in that: In step 2, the high-speed shearing time is 30 min to 60 min, the high-speed shearing speed is 6000 r / min to 12000 r / min, the ultrasonic treatment time is 20 min to 90 min, and the standing time is 1 h to 24 h.

8. The method for preparing a composite solvent cerium-based polishing liquid according to claim 1, characterized in that: The particle size D50 of the CeO2 abrasive in the slurry in step 2 is 400nm to 600nm.

9. The method for preparing a composite solvent cerium-based polishing liquid according to claim 1, characterized in that: In step 3, the pH regulator is ammonia water, and the oxidant is hydrogen peroxide.

10. A composite solvent cerium-based polishing liquid, characterized in that: The method is prepared by any one of claims 1 to 9.