Environment-friendly lithium-manganese battery sealant and preparation method thereof

By using the ratio of polyisoprene rubber and other components, a lithium manganese battery sealant without aromatics was prepared, which solved the problem of insufficient toluene odor and performance in the existing lithium manganese battery sealant, and realized the sealant The environmentally friendly improvements have excellent weather resistance and airtightness, which are suitable for industrial production.

CN118978878AInactive Publication Date: 2024-11-19GUANGZHOU XINDI IND TECHNOLOGY CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410943635.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-15
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing lithium manganese battery sealant contains a large amount of toluene, which leads to a strong odor during the production process, poses a threat to workers' health, and has insufficient performance, making it difficult to meet the technical indicators of lithium manganese batteries.

Method used

A sealant without aromatic solvents is prepared by specific ratios and process treatments. , has excellent electrolyte resistance, heat resistance, humidity resistance and low temperature resistance.

Benefits of technology

The prepared sealant has no aromatic odor, has good bonding properties and airtightness, can withstand temperatures above 85℃, and has good low temperature resistance. It is suitable for packaging of lithium manganese batteries, simplifies the process flow and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004944956680000061
    Figure BDA0004944956680000061
  • Figure BDA0004944956680000071
    Figure BDA0004944956680000071
Patent Text Reader

Abstract

The invention discloses an environment-friendly lithium-manganese battery sealant which is prepared by taking polyisoprene rubber as a main component and adding tackifying resin, hydrogenated saturated polybutylene, white carbon black, dearomatized solvent oil and blue dye. The sealant does not contain an aromatic solvent, is small in smell, and is an environment-friendly sealant for the lithium-manganese battery; the sealant is insoluble in electrolyte of the lithium-manganese battery, has good bonding performance on metal and a sealing ring, generates a compact flexible protection layer, and effectively improves the barrier property of the sealing ring on water vapor and air and the properties of high and low temperature resistance, impact resistance, acid and alkali corrosion resistance and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an environmentally friendly lithium manganese battery sealant and a preparation method thereof. Background Art

[0002] Lithium manganese battery, as the most affordable and safest type of lithium primary battery, uses high potential and high specific energy metal lithium as the negative electrode active material, and the electrolyte is based on inorganic salt lithium perchlorate, dissolved in a mixed organic solvent of propylene carbonate (PC) and 1,2-dimethoxyethane (DME). The battery is exquisitely designed, thin and short, with high capacity and stable discharge curve, so it is widely used in high-tech products such as motherboards as a backup power source for memory. In addition, cylindrical lithium batteries have become the preferred choice in the camera battery market due to their high capacity, low internal resistance and instantaneous high current output.

[0003] In the production process of lithium-manganese batteries, sealant is a key auxiliary material, and its sealing effect has a significant impact on the final performance of the battery. The sealing process of lithium-manganese batteries involves immersing the sealing ring in lithium-manganese battery sealant, followed by drying in preparation for subsequent sealing. At present, the main lithium-manganese battery sealant products on the domestic market are produced by a limited company in Harbin. The sealant contains a large amount of toluene, which will produce a strong odor during the immersion and drying of the sealing ring, posing a serious threat to the health of workers. Summary of the invention

[0004] In view of the deficiencies in the prior art, the purpose of the present invention is to provide an environmentally friendly lithium manganese battery sealant and a preparation method thereof, which is prepared without using aromatic hydrocarbon solvents and has excellent electrolyte resistance, heat resistance, moisture resistance, and low temperature resistance, and can meet the technical indicators of lithium manganese battery sealants.

[0005] The technical solution adopted by the present invention to solve its technical problem is:

[0006] The invention discloses an environmentally friendly lithium manganese battery sealant, which comprises the following components: polyisoprene rubber, tackifying resin, hydrogenated saturated polybutene, thixotropic agent, dearomatized solvent and dye.

[0007] Preferably, the composition comprises the following components in percentage by weight: polyisoprene rubber: 10 to 20 parts, tackifying resin: 5 to 20 parts, hydrogenated saturated polybutene: 3 to 10 parts, thixotropic agent: 0.5 to 2 parts, dearomatizing solvent: 65 to 80 parts, and dye: 0.05 to 0.5 parts.

[0008] Preferably, the following components are included in percentage by weight: polyisoprene rubber: 15 parts, tackifying resin: 10 parts, hydrogenated saturated polybutene: 3 parts, thixotropic agent: 1 part, dearomatization solvent: 65 parts, dye: 0.1 parts.

[0009] Preferably, the following components are included in percentage by weight: polyisoprene rubber: 12 parts, tackifying resin: 12 parts, hydrogenated saturated polybutene: 4 parts, thixotropic agent: 1 part, dearomatization solvent: 60 parts, dye: 0.1 parts.

[0010] Preferably, the following components are included in percentage by weight: polyisoprene rubber: 17 parts, tackifying resin: 8 parts, hydrogenated saturated polybutene: 4 parts, thixotropic agent: 1 part, dearomatization solvent: 70 parts, dye: 0.1 parts.

[0011] Preferably, the tackifying resin is hydrogenated C5 petroleum resin.

[0012] Preferably, the number average molecular weight of the hydrogenated saturated polybutene is 1000-1500.

[0013] Preferably, the thixotropic agent is fumed silica or diatomaceous earth.

[0014] Preferably, the dearomatization solvent is a D30 dearomatization solvent.

[0015] Another technical problem to be solved by the present invention is to provide a method for preparing an environmentally friendly lithium manganese battery sealant, comprising the following steps:

[0016] Cut the polyisoprene rubber into pieces using a vertical single-knife rubber cutter, add the pieces into a stirring and dissolving tank, add a dearomatization solvent, stir and dissolve, and keep the seal to prevent the solvent from volatilizing, thereby obtaining a polyisoprene rubber solution;

[0017] Add tackifying resin, hydrogenated saturated polybutene, thixotropic agent and blue dye into the polyisoprene rubber solution, stir evenly, and then add dearomatization solvent to adjust the viscosity.

[0018] Polyisoprene rubber: This material has excellent weather resistance and corrosion resistance, exhibits excellent low gas permeability, low temperature flexibility and high electrical insulation, and can withstand lithium manganese battery electrolyte. The recommended usage range is 10 to 20 parts (by weight).

[0019] Tackifying resin: Hydrogenated C5 petroleum resin is preferred, and its main function is to improve the bonding strength. Traditional tackifying resins have poor solubility in dearomatized solvents and are prone to precipitation during the preparation process, which in turn affects the performance of lithium manganese batteries. After careful selection, the present invention determines to use hydrogenated C5 petroleum resin as a tackifying resin to significantly improve the comprehensive performance of the sealant. The recommended dosage range is 5 to 20 parts (by weight).

[0020] Hydrogenated saturated polybutene: As a plasticizer, its main function is to improve the adhesion and viscosity of the material and enhance the flexibility of the adhesive layer, thereby optimizing the sealing performance of the sealing material. Hydrogenated saturated polybutene with a number average molecular weight of 1000-1500 is preferred. The recommended dosage range is 3 to 10 parts (by weight).

[0021] Thixotropic agent: It uses materials such as fumed silica and diatomaceous earth to enhance the thixotropy and sag resistance of the sealant. The recommended dosage is 0.5 to 2 parts (by weight).

[0022] Dearomatization solvent: D30 dearomatization solvent is used. It is a solvent oil that has been treated with hydrogenation and refining. The aromatic hydrocarbons are effectively removed, the odor is small, and it meets environmental protection requirements. The recommended dosage range is 65 to 80 parts (by weight).

[0023] Blue dye: This dye is used to identify whether the lithium manganese battery has been coated with glue or has a glue break, to ensure product quality. The recommended dosage is 0.05 to 0.5 parts (by weight).

[0024] The beneficial effects of the present invention are:

[0025] The lithium manganese battery sealant of the present invention does not contain aromatic solvents and has little odor, and is an environmentally friendly lithium manganese battery sealant; the sealant is insoluble in lithium manganese battery electrolyte, has good bonding properties to metals and sealing rings, has good air tightness, can withstand temperatures above 85°C, and has good low temperature resistance. Moreover, it has good droop resistance during use, will not draw, and has fast film formation; at the same time, the preparation method of the sealant is simple, the process flow is short, and it is suitable for industrial production. DETAILED DESCRIPTION

[0026] The principles and features of the present invention are described below, and the examples are only used to explain the present invention and are not used to limit the scope of the present invention. The present invention is described more specifically by way of example in the following paragraphs. According to the following description and claims, the advantages and features of the present invention will become clearer.

[0027] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.

[0028] The following is the result of rewriting in a rigorous, stable, rational and official language style:

[0029] Example 1

[0030] A method for preparing an environmentally friendly lithium manganese battery sealant comprises the following steps:

[0031] To prepare a polyisoprene rubber solution, 15 parts of polyisoprene rubber were weighed, cut into pieces in a vertical single-blade rubber cutter, and added to a stirring and dissolving tank. Subsequently, 65 parts of D30 dearomatization solvent were added, and stirring and dissolving were continued for 5 hours. To ensure safe operation, the whole process must be kept sealed to prevent solvent volatilization, thereby obtaining a polyisoprene rubber solution.

[0032] Add 10 parts of hydrogenated C5 petroleum resin, 3 parts of hydrogenated saturated polybutene, 1 part of fumed silica and 0.1 part of blue dye to the prepared polyisoprene rubber solution. Stir again for 2 hours until all ingredients are completely dissolved. Then, add 6 parts of D30 dearomatization solvent, adjust the viscosity of the sealant to an appropriate level, and complete the discharging operation.

[0033] Example 2

[0034] A method for preparing an environmentally friendly lithium manganese battery sealant comprises the following steps:

[0035] To prepare a polyisoprene rubber solution, 12 parts of polyisoprene rubber were weighed, cut and added to a stirring and dissolving tank, followed by adding 60 parts of D30 dearomatization solvent, stirring and dissolving for 5 hours. The whole process was kept sealed to ensure safe operation and non-volatile solvent, thereby obtaining a polyisoprene rubber solution.

[0036] 12 parts of hydrogenated C5 petroleum resin, 4 parts of hydrogenated saturated polybutene, 1 part of fumed silica and 0.1 part of blue dye were added to the solution and stirred for 2 hours until completely dissolved. Subsequently, 11 parts of D30 dearomatization solvent were added to adjust the sealant viscosity to the standard value and the discharge was completed.

[0037] Example 3

[0038] A method for preparing an environmentally friendly lithium manganese battery sealant comprises the following steps:

[0039] Prepare polyisoprene rubber solution, weigh 17 parts of polyisoprene rubber, cut and add to the stirring dissolution tank, then add 70 parts of D30 dearomatization solvent, continue stirring and dissolving for 5 hours. Keep sealed during the whole process to ensure safe operation and non-volatile solvent.

[0040] 8 parts of hydrogenated C5 petroleum resin, 4 parts of hydrogenated saturated polybutene, 1 part of fumed silica and 0.1 part of blue dye were added to the solution and stirred for 2 hours until they were completely dissolved. Subsequently, 10 parts of D30 dearomatization solvent were added to adjust the sealant viscosity to an appropriate level and the discharge was completed.

[0041] Example 4

[0042] A method for preparing an environmentally friendly lithium manganese battery sealant comprises the following steps:

[0043] Prepare polyisoprene rubber solution, weigh 15 parts of polyisoprene rubber, cut and add to the stirring dissolution tank, then add 65 parts of D30 dearomatization solvent, and continue stirring and dissolving for 5 hours. Keep it sealed throughout the process to ensure safe operation and non-volatile solvent.

[0044] 15 parts of hydrogenated C5 petroleum resin, 5 parts of hydrogenated saturated polybutene, 1 part of fumed silica and 0.1 part of blue dye were added to the prepared solution and stirred for 2 hours until all the components were completely dissolved. Subsequently, 9 parts of D30 dearomatization solvent were added to adjust the viscosity of the sealant to the required level and the discharging operation was completed.

[0045] Example 5

[0046] A method for preparing an environmentally friendly lithium manganese battery sealant comprises the following steps:

[0047] Prepare polyisoprene rubber solution, weigh 20 parts of polyisoprene rubber, cut and add to the stirring dissolution tank, then add 70 parts of D30 dearomatization solvent, and continue stirring and dissolving for 5 hours. Keep it sealed throughout the process to ensure safe operation and non-volatile solvent.

[0048] 20 parts of hydrogenated C5 petroleum resin, 10 parts of hydrogenated saturated polybutene, 2 parts of fumed silica and 0.5 parts of blue dye were added to the prepared solution and stirred for 2 hours until all the components were completely dissolved. Subsequently, 10 parts of D30 dearomatization solvent were added to adjust the viscosity of the sealant to the required level and the discharging operation was completed.

[0049] Example 6

[0050] A method for preparing an environmentally friendly lithium manganese battery sealant comprises the following steps:

[0051] Prepare polyisoprene rubber solution, weigh 10 parts of polyisoprene rubber, cut and add to the stirring dissolution tank, then add 60 parts of D30 dearomatization solvent, and continue stirring and dissolving for 5 hours. Keep it sealed throughout the process to ensure safe operation and non-volatile solvent.

[0052] Add 5 parts of hydrogenated C5 petroleum resin, 3 parts of hydrogenated saturated polybutene, 0.5 parts of fumed silica and 0.05 parts of blue dye to the prepared solution, and continue stirring for 2 hours until all the ingredients are completely dissolved. Then, add 5 parts of D30 dearomatization solvent, adjust the viscosity of the sealant to the required level, and complete the discharging operation.

[0053] Experimental example

[0054] Experimental subjects

[0055] The lithium manganese battery sealant prepared in Example 1-6;

[0056] The lithium manganese battery sealants currently on the market;

[0057] Peel strength test:

[0058] First, the sealant is evenly and accurately applied to a standard test piece to ensure the consistency and uniformity of the coating. The sealant is then allowed to cure naturally at room temperature for 24 hours to ensure that it reaches a stable performance state.

[0059] After curing, the test piece is fixed on a professional tensile testing machine to ensure that it is firmly fixed and accurately positioned. Then, the test piece is stretched at a predetermined fixed speed until the sealant is peeled off. During this process, the maximum force required is recorded to accurately evaluate the peel strength.

[0060] Shear strength test:

[0061] In another test, the sealant was evenly applied to two overlapping metal panels and again, the sealant was allowed to cure for 24 hours under the specified conditions.

[0062] After curing, the two overlapping metal plates are placed in a tensile testing machine and their positions are stable and accurate. Then, a vertical force is applied to the bonding interface until the bond breaks. During this process, the maximum force at break is recorded to evaluate the shear strength.

[0063] According to the above test, the results are shown in Table 1 below.

[0064] Table 1

[0065]

[0066] The peel strength test analysis shows that according to the existing data, the embodiment sealant generally shows a slightly higher performance in peel strength than similar products on the market. This data indicates that the embodiment sealant may have better interfacial adhesion performance. In the shear strength test, the embodiment sealant also showed its excellent performance, which is probably attributed to the precise formulation of its chemical formula and the optimization of curing conditions. In summary, the performance of the embodiment sealant in both peel strength and shear strength exceeds that of some similar products on the market, which provides strong support for its potential advantages in specific application scenarios (such as lithium manganese battery packaging).

[0067] Experimental Example 2

[0068] Experimental subjects

[0069] The lithium manganese battery sealant prepared in Example 1-6;

[0070] The lithium manganese battery sealants currently on the market;

[0071] Leak test

[0072] First, sealant is precisely applied to the interface of the sealed container to ensure that the interface is completely sealed. Subsequently, gas at a specific pressure that meets the specification requirements is applied inside the container. Next, a professional leak detector is used to conduct a comprehensive inspection of the sealed parts to determine whether there is any gas escape. During the inspection process, the exact time and location of any leaks must be recorded in detail to provide accurate data for subsequent analysis.

[0073] Air pressure drop test

[0074] A predetermined air pressure value is applied in a closed system to ensure that the internal pressure of the system reaches a stable state. Subsequently, after a set time interval, professional equipment is used to accurately detect the pressure changes in the system. Through detailed analysis of the pressure drop data, the airtightness performance of the sealant is scientifically evaluated, providing a strong basis for improving product quality.

[0075] The test results are shown in Table 2 below.

[0076] Table 2

[0077]

[0078] According to the experimental data, the tested sealants of the examples showed a significantly longer leakage start time compared to the sealants circulating in the market. It is particularly worth mentioning that Examples 1-6 did not show any leakage during the 72-hour test period, which fully demonstrated their excellent sealing performance.

[0079] During the 24-hour test period, the pressure drop of the embodiment sealant was relatively small, which significantly demonstrated its excellent airtightness. At the same time, the commercial sealant showed a higher pressure drop percentage under the same test conditions, which may be due to differences in material properties or insufficient sealing effect.

[0080] Based on the results of the leakage test and the air pressure drop test, the sealants of the embodiments all showed high performance. This is mainly due to its optimized chemical composition and excellent sealing effect. Therefore, these test results provide strong support for the application of the sealants of the embodiments in the field of lithium manganese batteries, and may have an important impact on the overall safety and efficiency of such batteries.

[0081] The above embodiments of the present invention are not intended to limit the protection scope of the present invention, and the implementation modes of the present invention are not limited thereto. All other modifications, replacements or changes made to the above structures of the present invention based on the above contents of the present invention, in accordance with common technical knowledge and customary means in the art, without departing from the above basic technical ideas of the present invention, should fall within the protection scope of the present invention.

Claims

1. An environmentally friendly lithium manganese battery sealant, characterized in that: The invention comprises the following ingredients: polyisoprene rubber, tackifying resin, hydrogenated saturated polybutene, thixotropic agent, dearomatization solvent and dye.

2. The environmentally friendly lithium manganese battery sealant according to claim 1, characterized in that: The invention comprises the following components in percentage by weight: polyisoprene rubber: 10 to 20 parts, tackifying resin: 5 to 20 parts, hydrogenated saturated polybutene: 3 to 10 parts, thixotropic agent: 0.5 to 2 parts, dearomatization solvent: 65 to 80 parts, and dye: 0.05 to 0.5 parts.

3. The environmentally friendly lithium manganese battery sealant according to claim 1 or 2, characterized in that: The invention comprises the following components in percentage by weight: polyisoprene rubber: 15 parts, tackifying resin: 10 parts, hydrogenated saturated polybutene: 3 parts, thixotropic agent: 1 part, dearomatization solvent: 65 parts, and dye: 0.1 parts.

4. The environmentally friendly lithium manganese battery sealant according to claim 1 or 2, characterized in that: The invention comprises the following components in percentage by weight: polyisoprene rubber: 12 parts, tackifying resin: 12 parts, hydrogenated saturated polybutene: 4 parts, thixotropic agent: 1 part, dearomatization solvent: 60 parts, and dye: 0.1 parts.

5. The environmentally friendly lithium manganese battery sealant according to claim 1 or 2, characterized in that: The invention comprises the following components in percentage by weight: polyisoprene rubber: 17 parts, tackifying resin: 8 parts, hydrogenated saturated polybutene: 4 parts, thixotropic agent: 1 part, dearomatization solvent: 70 parts, and dye: 0.1 parts.

6. The environmentally friendly lithium manganese battery sealant according to claim 1 or 2, characterized in that: The tackifying resin is a hydrogenated C5 petroleum resin.

7. The environmentally friendly lithium manganese battery sealant according to claim 6, characterized in that: The number average molecular weight of the hydrogenated saturated polybutene is 1000-1500.

8. The environmentally friendly lithium manganese battery sealant according to claim 7, characterized in that: The thixotropic agent is fumed silica or diatomaceous earth.

9. The environmentally friendly lithium manganese battery sealant according to claim 8, characterized in that: The dearomatization solvent is D30 dearomatization solvent.

10. A method for preparing an environmentally friendly lithium manganese battery sealant, characterized in that: The following steps are involved: Cut the polyisoprene rubber into pieces using a vertical single-knife rubber cutter, add the pieces into a stirring and dissolving tank, add a dearomatization solvent, stir and dissolve, and keep the seal to prevent the solvent from volatilizing, thereby obtaining a polyisoprene rubber solution; Add tackifying resin, hydrogenated saturated polybutene, thixotropic agent and blue dye into the polyisoprene rubber solution, stir evenly, and then add dearomatization solvent to adjust the viscosity.

Citation Information

Patent Citations

  • Lithium powder anode

    CN105188990A

  • Lithium-manganese battery sealant and preparation method thereof

    CN114426803A