High-temperature-resistant and high-humidity-resistant optical pressure-sensitive adhesive as well as preparation method and protective film thereof
Through the compounding and staged reaction of raw materials such as acrylate monomers, optical pressure-sensitive adhesives that are resistant to high temperature and high humidity are prepared, which solves the problem of insufficient performance of existing optical pressure-sensitive adhesives in high temperature and high humidity environments, and achieves good results The bonding and photoelectric properties are suitable for the production of LCD panels.
Patent Information
- Application Number
- CN202411046528.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
AI Technical Summary
The existing optical pressure-sensitive adhesives are insufficient in high temperature and high humidity environments, making it difficult to meet the high requirements of the polarizer of the liquid crystal display panel.
Using the combination of raw materials such as acrylate monomers, functional monomers, initiators, silane coupling agents, etc., to prepare high temperature and high humidity-resistant optical pressure-sensitive adhesives by carefully designing the types and ratios of raw materials, and adopting staged reactions The preparation method of mixing with components is formed to form a film with good adhesive properties and photoelectric properties.
It realizes good bonding performance, high temperature resistance, high humidity performance and excellent photoelectric performance of optical pressure sensitive adhesive. It is suitable for the production and use of liquid crystal display panels. It has a simple and easy-to-control preparation method, high production efficiency, low cost, and suitable for scale Chemical production.
Smart Images

Figure BDA0004973630330000101
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of adhesives, and in particular to an optical pressure-sensitive adhesive resistant to high temperature and high humidity and a preparation method thereof. Background Art
[0002] Pressure-sensitive adhesive is a type of adhesive that can quickly bond to a substrate under low pressure. It does not require solvent volatilization or chemical reaction for bonding, and bonding can be carried out at room temperature. It can be easily and quickly attached to the surface of the adhered object, and can be easily peeled off from the surface of the adhered object without contaminating the adhered object, playing a role in bonding and protecting the adhered object.
[0003] The polarizer on the liquid crystal display panel is an important component of the liquid crystal panel, mainly for polarization. It needs to be attached with a protective film during processing, handling, and assembly, mainly to avoid surface contamination and scratches on the polarizer. In actual production and application, there are very high performance requirements for the polarizer protective film. The role of optical pressure-sensitive adhesive is to attach the polarizer to the liquid crystal display glass panel. The performance of the optical pressure-sensitive adhesive has an important influence on the bonding and processing performance of the polarizer. Therefore, it is of great significance to prepare a pressure-sensitive adhesive and polarizer protective film with good optoelectronic properties and bonding properties, and high high temperature and high humidity stability. Summary of the invention
[0004] In order to solve the above-mentioned deficiencies of the prior art, one of the objects of the present invention is to provide an optical pressure-sensitive adhesive resistant to high temperature and high humidity, which has good bonding properties, high temperature resistance, high humidity resistance and better photoelectric properties to meet practical application requirements.
[0005] Another object of the present invention is to provide a method for preparing an optical pressure-sensitive adhesive resistant to high temperature and high humidity. The method for preparing the optical pressure-sensitive adhesive resistant to high temperature and high humidity has a simple and easy-to-control process, high production efficiency, low production cost, and the obtained pressure-sensitive adhesive product has stable quality and excellent comprehensive performance, and is suitable for large-scale production.
[0006] Another object of the present invention is to provide a polarizer protective film, wherein the polarizer protective film has the above-mentioned optical pressure-sensitive adhesive layer.
[0007] The objective of the present invention is achieved through the following technical scheme: an optical pressure-sensitive adhesive resistant to high temperature and high humidity, comprising component A and component B, wherein component A comprises the following raw materials in parts by weight: 80-90 parts of acrylate monomers, 0.1-5 parts of functional monomers, 0.2-0.5 parts of initiators, 1-10 parts of silane coupling agents, 100-120 parts of solvents, and 1-4 parts of auxiliary agents; and component B comprises the following raw materials in parts by weight: 1-3 parts of cross-linking agents and 1-2.5 parts of curing accelerators.
[0008] Furthermore, the acrylic acid ester monomer is composed of methyl acrylate, butyl acrylate, and aromatic ring-containing (meth) alkyl acrylate in a weight ratio of 1:5-10:2-5. In the present invention, aromatic ring-containing (meth) alkyl acrylate refers to aromatic ring-containing methacrylate and aromatic ring-containing alkyl acrylate.
[0009] Furthermore, the aromatic ring-containing alkyl (meth)acrylate is at least one of phenoxyethyl acrylate, benzyl acrylate, phenoxydiethylene glycol acrylate, phenoxyethyl methacrylate and benzyl methacrylate.
[0010] Furthermore, the functional monomer is at least one of acrylic acid, hydroxyethyl acrylate, hydroxybutyl acrylate, methacrylic acid, hydroxyethyl acrylate, hydroxybutyl methacrylate and diacetone acrylamide.
[0011] Furthermore, the functional monomer is composed of acrylic acid, hydroxyethyl acrylate and diacetone acrylamide in a weight ratio of 1:1-3:0.2-0.5.
[0012] The invention compound raw materials such as methyl acrylate, butyl acrylate, acrylic acid, hydroxyethyl acrylate and diacetone acrylamide, and carefully control the dosage ratio of each raw material, so that each raw material can be well matched. The introduction of aromatic ring (meth) alkyl acrylate monomer can suppress the problem that the surface resistivity of the optical pressure-sensitive adhesive film increases with time under high temperature and high humidity environment. At the same time, the introduction of aromatic ring can meet the durability requirement and improve the light leakage problem, and comprehensively meet the photoelectric performance required by the optical pressure-sensitive adhesive. The introduction of diacetone acrylamide is helpful to improve the thermal stability, peeling strength and holding force of the optical pressure-sensitive adhesive. The amide group contained in the diacetone acrylamide can form hydrogen bonds and physical crosslinking points, thereby increasing the intermolecular force. At the same time, it is prevented that the addition amount of diacetone acrylamide is too large, which leads to an increase in the cohesive force of the pressure-sensitive adhesive system and an increase in viscosity, and reduces the fluidity and initial adhesion of the pressure-sensitive adhesive layer.
[0013] Furthermore, the solvent is at least one of ethyl acetate and toluene.
[0014] Furthermore, the initiator is at least one of a peroxide initiator and an azo initiator.
[0015] Furthermore, the peroxide initiator is at least one of lauroyl peroxide and tert-butyl benzoyl peroxide. The azo initiator is at least one of azobisisobutyronitrile and azobisisoheptylnitrile.
[0016] Furthermore, the silane coupling agent is at least one of γ-glycidyloxypropyltrimethoxysilane and γ-(methacryloyloxy)propyltrimethoxysilane.
[0017] Furthermore, each portion of the auxiliary agent includes the following raw materials in parts by weight: 0.5-2 parts of antioxidant and 0.5-2 parts of defoaming agent.
[0018] Furthermore, the cross-linking agent is at least one of an isocyanate cross-linking agent, an aziridine cross-linking agent and a metal chelate cross-linking agent.
[0019] Furthermore, the curing accelerator is composed of acetylacetonate metal salt and acetylacetone in a weight ratio of 1:0.1-0.2. The acetylacetonate metal salt is at least one of aluminum acetylacetonate and zinc acetylacetonate.
[0020] Furthermore, the method for preparing the high temperature and high humidity resistant optical pressure sensitive adhesive comprises the following steps:
[0021] (1) preparing component A and component B respectively;
[0022] The preparation method of the A component comprises the following steps:
[0023] (A1) under nitrogen protection, adding part of the solvent into a reaction vessel, stirring and heating to 68-82° C., and keeping the temperature for 20-40 minutes; mixing methyl acrylate, butyl acrylate, aromatic ring-containing (meth) alkyl acrylate, diacetone acrylamide and part of the initiator to obtain a mixture I;
[0024] (A2) adding part of the mixture I to a reaction vessel, and mixing evenly with the solvent treated in step (A1), the reaction temperature is 68-82° C., and the reaction time is 30-60 min;
[0025] (A3) mixing hydroxyethyl acrylate, the remaining mixture I, a silane coupling agent and part of the solvent to obtain a mixture II; dropping the mixture II into a reaction vessel, keeping the temperature at 68-82° C., adding the remaining initiator and part of the solvent, and dropping the mixture II within 150-210 minutes;
[0026] (A4) After the mixture II is added dropwise, the mixture is kept warm for 180-240 minutes, and then the auxiliary agent and the remaining solvent are added, and the mixture is stirred evenly to obtain the mixture. The reaction solution is cooled to room temperature, and then added to obtain component A; the component A is adjusted to have a solid content of 15-35%;
[0027] The preparation method of the B component comprises the following steps:
[0028] The crosslinking agent and the curing accelerator are uniformly mixed according to the weight ratio to prepare component B;
[0029] (2) Mix component A and component B evenly.
[0030] The present invention adopts the above-mentioned preparation method to prepare an acrylic pressure-sensitive adhesive, first reacting part of the monomers with part of the initiator in a reaction vessel for a period of time, and then continuing to add the remaining monomers, silane coupling agents and initiators, and reacting in stages, which helps to improve the overall performance of the copolymer. Before the pressure-sensitive adhesive of the present invention is in an unused state, component A and component B are prepared separately, and when used, component A mainly composed of acrylic copolymer is mixed with a component containing a cross-linking agent to prepare a polarizer protective film, which is convenient for storage and transportation, and the prepared polarizer protective film has good thermal stability and adhesion, and there is no residual glue after peeling, and the photoelectric properties meet the production and use requirements.
[0031] The present invention also provides a polarizer protective film, comprising a base film and a pressure-sensitive adhesive layer arranged on the surface of the base film, wherein the pressure-sensitive adhesive layer is made of the above-mentioned aging-resistant pressure-sensitive adhesive.
[0032] The present invention also provides a method for preparing the above-mentioned polarizer protective film, comprising the following steps: mixing component A and component B evenly, then coating them on the surface of the base film, drying at 110-120°C for 3-10 minutes, and then maintaining at 55-65°C for 20-30 hours.
[0033] The beneficial effects of the present invention are as follows: the optical pressure-sensitive adhesive resistant to high temperature and humidity provided by the present invention is prepared by compounding raw materials such as acrylate monomers, functional monomers, initiators, silane coupling agents, and carefully designing the raw material types and ratios of acrylate monomers and functional monomers to obtain an optical pressure-sensitive adhesive resistant to high temperature and humidity, and further using the above-mentioned aging-resistant optical pressure-sensitive adhesive to prepare an optical pressure-sensitive adhesive; the optical pressure-sensitive adhesive has good bonding performance, high temperature resistance, high humidity performance and better photoelectric performance, meeting the needs of practical applications. The preparation method of the optical pressure-sensitive adhesive resistant to high temperature and humidity is simple and easy to control, has high production efficiency, low production cost, and the obtained pressure-sensitive adhesive product has stable quality and excellent comprehensive performance, and is suitable for large-scale production. DETAILED DESCRIPTION
[0034] In order to facilitate the understanding of those skilled in the art, the present invention is further described below in conjunction with embodiments, and the contents mentioned in the implementation modes are not intended to limit the present invention.
[0035] In an embodiment of the present invention, a high temperature and high humidity resistant optical pressure-sensitive adhesive comprises component A and component B, wherein component A comprises the following raw materials in parts by weight: 80-90 parts of acrylate monomer, 0.1-5 parts of functional monomer, 0.2-0.5 parts of initiator, 1-10 parts of silane coupling agent, 100-120 parts of solvent, and 1-4 parts of auxiliary agent; and component B comprises the following raw materials in parts by weight: 1-3 parts of cross-linking agent and 1-2.5 parts of curing accelerator.
[0036] In some embodiments of the present invention, the acrylic acid ester monomers are composed of methyl acrylate, butyl acrylate and aromatic ring-containing alkyl (meth)acrylate in a weight ratio of 1:5-10:2-5.
[0037] In some embodiments of the present invention, the aromatic ring-containing alkyl (meth)acrylate is at least one of phenoxyethyl acrylate, benzyl acrylate, phenoxydiethylene glycol acrylate, phenoxyethyl methacrylate and benzyl methacrylate.
[0038] In some embodiments of the present invention, the functional monomer is at least one of acrylic acid, hydroxyethyl acrylate, hydroxybutyl acrylate, methacrylic acid, hydroxyethyl acrylate, hydroxybutyl methacrylate and diacetone acrylamide.
[0039] In some embodiments of the present invention, the functional monomer is composed of acrylic acid, hydroxyethyl acrylate and diacetone acrylamide in a weight ratio of 1:1-3:0.2-0.5.
[0040] In some embodiments of the present invention, the solvent is at least one of ethyl acetate and toluene.
[0041] In some embodiments of the present invention, the initiator is at least one of a peroxide initiator and an azo initiator.
[0042] In some embodiments of the present invention, the peroxide initiator is at least one of lauroyl peroxide and tert-butyl benzoyl peroxide. The azo initiator is at least one of azobisisobutyronitrile and azobisisoheptylnitrile.
[0043] In some embodiments of the present invention, the silane coupling agent is at least one of γ-glycidyloxypropyltrimethoxysilane and γ-(methacryloxy)propyltrimethoxysilane.
[0044] In some embodiments of the present invention, each portion of the auxiliary agent comprises the following raw materials in parts by weight: 0.5-2 parts of antioxidant and 0.5-2 parts of defoaming agent.
[0045] In some embodiments of the present invention, the antioxidant is at least one of antioxidant 1010, antioxidant 168 and antioxidant 1076. The defoaming agent is an organic silicon defoaming agent.
[0046] In some embodiments of the present invention, the crosslinking agent is at least one of an isocyanate crosslinking agent, an aziridine crosslinking agent, and a metal chelate crosslinking agent.
[0047] In some embodiments of the present invention, the curing accelerator is composed of acetylacetone metal salt and acetylacetone in a weight ratio of 1:0.1-0.2.
[0048] In some embodiments of the present invention, the method for preparing the high temperature and high humidity resistant optical pressure sensitive adhesive comprises the following steps:
[0049] (1) preparing component A and component B respectively;
[0050] The preparation method of the A component comprises the following steps:
[0051] (A1) under nitrogen protection, 1 / 3-1 / 2 of the solvent is added to a reaction vessel, stirred and heated to 68-82° C., and kept warm for 20-40 minutes; methyl acrylate, butyl acrylate, aromatic ring-containing (meth) alkyl acrylate, diacetone acrylamide and 1 / 3-1 / 2 of the initiator are mixed uniformly to obtain a mixture I;
[0052] (A2) adding 1 / 2-2 / 3 of the mixture I into a reaction vessel, mixing evenly with the solvent treated in step (A1), controlling the temperature at 68-82° C., and reacting for 30-60 min;
[0053] (A3) mixing hydroxyethyl acrylate, the remaining mixture I, a silane coupling agent and 1 / 6-1 / 3 of a solvent to obtain a mixture II; dropping the mixture II into a reaction vessel, keeping the temperature at 68-82° C., adding the remaining initiator and dropping 1 / 6-1 / 3 of the solvent, and completing the dropping of the mixture II within 150-210 min;
[0054] (A4) After the mixture II is added dropwise, the mixture is kept warm for 180-240 minutes, and then the auxiliary agent and the remaining solvent are added, and the mixture is stirred evenly to obtain the reaction solution. The reaction solution is cooled to room temperature, and then added to obtain component A;
[0055] The preparation method of the B component comprises the following steps:
[0056] The crosslinking agent and the curing accelerator are uniformly mixed according to the weight ratio to prepare component B;
[0057] (3) Mix component A and component B evenly.
[0058] In an embodiment of the present invention, a polarizer protective film includes a base film and a pressure-sensitive adhesive layer disposed on the surface of the base film, wherein the pressure-sensitive adhesive layer is made of the above-mentioned aging-resistant pressure-sensitive adhesive.
[0059] In some embodiments of the present invention, the method for preparing the polarizer protective film comprises the following steps: mixing component A and component B evenly, then coating the mixture on the surface of the base film, drying the mixture at 110-120° C. for 3-10 min, and then maintaining the mixture at 55-65° C. for 20-30 h.
[0060] Example 1
[0061] In the present embodiment, a high temperature and high humidity resistant optical pressure-sensitive adhesive includes component A and component B. Component A includes the following raw materials in parts by weight: 85 parts of acrylate monomer, 4 parts of functional monomer, 0.4 parts of initiator, 5 parts of silane coupling agent, 110 parts of solvent, and 3 parts of auxiliary agent; component B includes the following raw materials in parts by weight: 2 parts of cross-linking agent and 2 parts of curing accelerator.
[0062] Furthermore, the acrylic acid ester monomers are composed of methyl acrylate, butyl acrylate and aromatic ring-containing (meth) alkyl acrylate in a weight ratio of 1:7:3.
[0063] Furthermore, the aromatic ring-containing alkyl (meth)acrylate is composed of phenoxydiethylene glycol acrylate and phenoxyethyl acrylate in a weight ratio of 2:1.
[0064] Furthermore, the functional monomer is composed of acrylic acid, hydroxyethyl acrylate and diacetone acrylamide in a weight ratio of 1:2:0.4.
[0065] Furthermore, the solvent consists of ethyl acetate and toluene in a weight ratio of 1:0.5.
[0066] Furthermore, the initiator is lauroyl peroxide. The silane coupling agent is γ-glycidyloxypropyltrimethoxysilane.
[0067] Furthermore, each part of the auxiliary agent includes the following raw materials in parts by weight: 0.5-2 parts of antioxidant and 0.5-2 parts of defoamer. The antioxidant is antioxidant 1010. The defoamer is BYK028 organosilicon defoamer.
[0068] Furthermore, the crosslinking agent is hexamethylene diisocyanate trimer. The curing accelerator is composed of aluminum acetylacetonate and acetylacetone in a weight ratio of 1:0.15.
[0069] Furthermore, the method for preparing the high temperature and high humidity resistant optical pressure sensitive adhesive comprises the following steps:
[0070] (1) preparing component A and component B respectively;
[0071] The preparation method of the A component comprises the following steps:
[0072] (A1) under nitrogen protection, 1 / 3 of the solvent is added to a reaction vessel, stirred and heated to 70° C., and kept warm for 30 minutes; methyl acrylate, butyl acrylate, aromatic ring-containing (meth) alkyl acrylate, diacetone acrylamide and 1 / 2 of the initiator are mixed uniformly to obtain a mixture I;
[0073] (A2) adding 1 / 2 of the mixture I into a reaction vessel, mixing evenly with the solvent treated in step (A1), controlling the temperature at 70° C., and reacting for 40 min;
[0074] (A3) mixing hydroxyethyl acrylate, the remaining mixture I, a silane coupling agent and 1 / 3 of the solvent to obtain a mixture II; dropping the mixture II into a reaction vessel, keeping the temperature at 70° C., adding the remaining initiator and dropping 1 / 6 of the solvent, and the mixture II is added dropwise within 180 minutes;
[0075] (A4) After the mixture II is added dropwise, the mixture is kept warm for 210 minutes, and then the auxiliary agent and the remaining solvent are added, and the mixture is stirred evenly to obtain the reaction solution. The reaction solution is cooled to room temperature, and then component A is added;
[0076] The preparation method of the B component comprises the following steps:
[0077] The crosslinking agent and the curing accelerator are uniformly mixed according to the weight ratio to prepare component B;
[0078] (4) Mix component A and component B evenly.
[0079] In the present embodiment, a polarizer protective film includes a base film and a pressure-sensitive adhesive layer disposed on the surface of the base film, wherein the pressure-sensitive adhesive layer is made of the above-mentioned aging-resistant pressure-sensitive adhesive.
[0080] Furthermore, the preparation method of the polarizer protective film includes the following steps: mixing component A and component B evenly, then coating the mixture on the surface of the base film, drying the mixture at 115° C. for 6 minutes, and then maintaining the mixture at 60° C. for 24 hours.
[0081] Example 2
[0082] In the present embodiment, a high temperature and high humidity resistant optical pressure-sensitive adhesive includes component A and component B. Component A includes the following raw materials in parts by weight: 80 parts of acrylate monomer, 0.1 parts of functional monomer, 0.2 parts of initiator, 3 parts of silane coupling agent, 100 parts of solvent, and 2 parts of auxiliary agent; component B includes the following raw materials in parts by weight: 2 parts of cross-linking agent and 1.5 parts of curing accelerator.
[0083] Furthermore, the acrylic acid ester monomers are composed of methyl acrylate, butyl acrylate and aromatic ring-containing (meth) alkyl acrylate in a weight ratio of 1:5:2.
[0084] Furthermore, the aromatic ring-containing alkyl (meth)acrylate is composed of phenoxydiethylene glycol acrylate and benzyl methacrylate in a weight ratio of 1:1.
[0085] Furthermore, the functional monomer is composed of acrylic acid, hydroxyethyl acrylate and diacetone acrylamide in a weight ratio of 1:1:0.2.
[0086] Furthermore, the silane coupling agent is γ-(methacryloyloxy)propyltrimethoxysilane.
[0087] Furthermore, each part of the auxiliary agent includes the following raw materials in parts by weight: 0.5-2 parts of antioxidant and 0.5-2 parts of defoamer. The antioxidant is antioxidant 168. The defoamer is BYK028 silicone defoamer.
[0088] Furthermore, the crosslinking agent is hexamethylene diisocyanate trimer. The curing accelerator is composed of aluminum acetylacetonate and acetylacetone in a weight ratio of 1:0.15.
[0089] Furthermore, the method for preparing the high temperature and high humidity resistant optical pressure sensitive adhesive comprises the following steps:
[0090] (1) preparing component A and component B respectively;
[0091] The preparation method of the A component comprises the following steps:
[0092] (A1) under nitrogen protection, 1 / 3 of the solvent was added to a reaction vessel, stirred and heated to 70° C., and kept warm for 40 minutes; methyl acrylate, butyl acrylate, aromatic ring-containing (meth) alkyl acrylate, diacetone acrylamide and 1 / 2 of the initiator were mixed uniformly to obtain a mixture I;
[0093] (A2) adding 1 / 2 of the mixture I into a reaction vessel, mixing evenly with the solvent treated in step (A1), heating to 70° C., and reacting for 40 min;
[0094] (A3) mixing hydroxyethyl acrylate, the remaining mixture I, a silane coupling agent and 1 / 3 of the solvent to obtain a mixture II; dropping the mixture II into a reaction vessel, keeping the temperature at 70° C., adding the remaining initiator and dropping 1 / 6 of the solvent, and the mixture II is added dropwise within 150 minutes;
[0095] (A4) After the mixture II is added dropwise, the mixture is kept warm for 240 minutes, and then the auxiliary agent and the remaining solvent are added, and the mixture is stirred evenly to obtain the reaction solution. The reaction solution is cooled to room temperature, and then component A is added;
[0096] The preparation method of the B component comprises the following steps:
[0097] The crosslinking agent and the curing accelerator are uniformly mixed according to the weight ratio to prepare component B;
[0098] (5) Mix component A and component B evenly.
[0099] In the present embodiment, a polarizer protective film includes a base film and a pressure-sensitive adhesive layer disposed on the surface of the base film, wherein the pressure-sensitive adhesive layer is made of the above-mentioned aging-resistant pressure-sensitive adhesive.
[0100] The rest of the content of this embodiment is the same as that of Embodiment 1 and will not be repeated here.
[0101] Example 3
[0102] In the present embodiment, a high temperature and high humidity resistant optical pressure-sensitive adhesive includes component A and component B. Component A includes the following raw materials in parts by weight: 90 parts of acrylate monomer, 5 parts of functional monomer, 0.5 parts of initiator, 6 parts of silane coupling agent, 120 parts of solvent, and 3 parts of auxiliary agent; component B includes the following raw materials in parts by weight: 2 parts of cross-linking agent and 1 part of curing accelerator.
[0103] Furthermore, the acrylic acid ester monomer is composed of methyl acrylate, butyl acrylate and aromatic ring-containing (meth) alkyl acrylate in a weight ratio of 1:8:4.
[0104] Furthermore, the aromatic ring-containing alkyl (meth)acrylate is composed of phenoxydiethylene glycol acrylate and phenoxyethyl acrylate in a weight ratio of 2:1.
[0105] Furthermore, the functional monomer is composed of acrylic acid, hydroxyethyl acrylate and diacetone acrylamide in a weight ratio of 1:3:0.5.
[0106] Furthermore, the silane coupling agent is composed of γ-glycidyloxypropyltrimethoxysilane and γ-(methacryloyloxy)propyltrimethoxysilane in a weight ratio of 1:1.
[0107] Furthermore, the curing accelerator is composed of zinc acetylacetonate and acetylacetone in a weight ratio of 1:0.2.
[0108] Furthermore, the method for preparing the high temperature and high humidity resistant optical pressure sensitive adhesive comprises the following steps:
[0109] (1) preparing component A and component B respectively;
[0110] The preparation method of the A component comprises the following steps:
[0111] (A1) under nitrogen protection, 1 / 3 of the solvent was added to a reaction vessel, stirred and heated to 70° C., and kept warm for 20 minutes; methyl acrylate, butyl acrylate, aromatic ring-containing (meth) alkyl acrylate, diacetone acrylamide and 1 / 2 of the initiator were mixed uniformly to obtain a mixture I;
[0112] (A2) adding 1 / 2 of the mixture I into a reaction vessel, mixing evenly with the solvent treated in step (A1), controlling the temperature at 70° C., and reacting for 30 min;
[0113] (A3) mixing hydroxyethyl acrylate, the remaining mixture I, a silane coupling agent and 1 / 3 of the solvent to obtain a mixture II; dropping the mixture II into a reaction vessel, keeping the temperature at 70° C., adding the remaining initiator and a portion of the solvent, and dropping the mixture II within 210 minutes;
[0114] (A4) After the mixture II is added dropwise, the mixture is kept warm for 240 minutes, and then the auxiliary agent and the remaining solvent are added, and the mixture is stirred evenly to obtain the reaction solution. The reaction solution is cooled to room temperature, and then component A is added;
[0115] The preparation method of the B component comprises the following steps:
[0116] The crosslinking agent and the curing accelerator are uniformly mixed according to the weight ratio to prepare component B;
[0117] (6) Mix component A and component B evenly.
[0118] In the present embodiment, a polarizer protective film includes a base film and a pressure-sensitive adhesive layer disposed on the surface of the base film, wherein the pressure-sensitive adhesive layer is made of the above-mentioned aging-resistant pressure-sensitive adhesive.
[0119] The rest of the content of this embodiment is the same as that of Embodiment 1 and will not be repeated here.
[0120] Example 4
[0121] In the present embodiment, a high temperature and high humidity resistant optical pressure-sensitive adhesive includes component A and component B. Component A includes the following raw materials in parts by weight: 85 parts of acrylate monomer, 4 parts of functional monomer, 0.4 parts of initiator, 5 parts of silane coupling agent, 110 parts of solvent, and 3 parts of auxiliary agent; component B includes the following raw materials in parts by weight: 2 parts of cross-linking agent and 2 parts of curing accelerator.
[0122] Furthermore, the acrylic acid ester monomers are composed of methyl acrylate, butyl acrylate and aromatic ring-containing (meth) alkyl acrylate in a weight ratio of 1:6:3.
[0123] Furthermore, the aromatic ring-containing alkyl (meth)acrylate is composed of phenoxydiethylene glycol acrylate and benzyl acrylate in a weight ratio of 1:1.
[0124] Furthermore, the functional monomer is composed of acrylic acid, hydroxyethyl acrylate and diacetone acrylamide in a weight ratio of 1:2:0.3.
[0125] In the present embodiment, a polarizer protective film includes a base film and a pressure-sensitive adhesive layer disposed on the surface of the base film, wherein the pressure-sensitive adhesive layer is made of the above-mentioned aging-resistant pressure-sensitive adhesive.
[0126] The rest of the content of this embodiment is the same as that of Embodiment 1 and will not be repeated here.
[0127] Comparative Example 1
[0128] The difference between this comparative example and Example 1 is that in the preparation method of the A component, no aromatic ring-containing alkyl (meth)acrylate is added.
[0129] Comparative Example 2
[0130] The difference between this comparative example and Example 1 is that in the preparation method of component A, no diacetone acrylamide is added.
[0131] The polarizer protective films prepared in Examples 1-4 and Comparative Examples 1-2 were tested for performance, and the performance parameters are shown in Table 1 below:
[0132]
[0133] The rheological test experiment was conducted using TA's HR10 instrument with a temperature range of -50-200°C, a heating rate of 3°C / min, a frequency of 1HZ, and a φ: 8mm parallel plate fixture.
[0134] The peeling force test adopts the GB-T2792-1981 test standard.
[0135] The refractive index was measured using an Abbe refractometer from ATAGO, with a test wavelength of 589 nm and a test temperature of 25°C.
[0136] The resistance of the glue layer is tested by an antistatic value tester - an impedance tester, and the test temperature is 25°C and the humidity is 65%.
[0137] 60℃90%RH test: Cut the optical pressure-sensitive adhesive layer into 150×25mm, attach it to the surface of the polarizer, and put it into a constant temperature and humidity test box. After 500h of 60℃ and 90% humidity test, observe whether there are bubbles, detachment, or wrinkles on the surface of the polarizer. If there are no such phenomena, it is judged as qualified, otherwise it is judged as unqualified.
[0138] The initial adhesion is tested according to GB / T4582-2002 standard. The protective film is cut into samples with a size of 100mm×100mm and attached to the inclined surface of the instrument. Steel balls with specified numbers and different diameters are freely released from the standard line of the 30° inclined surface in order from large to small, until a steel ball with a certain number completely stops on the adhesive layer. This steel ball number is used to represent the initial adhesion performance of the pressure-sensitive adhesive layer of the protective film.
[0139] The 85℃ adhesion strength adopts the test standard of GB / T4851-2014. The protective film samples are cut into samples with a width of 25mm and a length of about 100mm, and attached to a stainless steel plate wiped clean with ethanol. The upper end is aligned with the standard line, and the excess part of the lower end is cut off. After rolling back and forth with a 2kg rubber roller for 3 times, it is placed for 20 minutes. The stainless steel plate with the sample is hung vertically on the test frame to prevent it from shaking, and a 1kg weight is hung underneath. The time it takes for the sample to fall under a temperature environment of 85℃ represents the adhesion strength of the pressure-sensitive adhesive layer of the protective film.
[0140] The high temperature and high humidity resistant optical pressure-sensitive adhesive provided by the present invention is prepared by compounding raw materials such as acrylate monomers, functional monomers, initiators, silane coupling agents, and carefully designing the raw material types and ratios of acrylate monomers and functional monomers to obtain the high temperature and high humidity resistant optical pressure-sensitive adhesive, and further using the above-mentioned aging-resistant optical pressure-sensitive adhesive to prepare the optical pressure-sensitive adhesive; the optical pressure-sensitive adhesive has good bonding performance, high temperature and high humidity resistance, and has better photoelectric performance, meeting the actual application requirements. The preparation method of the high temperature and high humidity resistant optical pressure-sensitive adhesive is simple and easy to control, has high production efficiency, low production cost, and the obtained pressure-sensitive adhesive product has stable quality and excellent comprehensive performance, and is suitable for large-scale production.
[0141] The above specific embodiments are further explanations of the technical solutions and beneficial effects of the present invention, and are not limitations of the implementation methods. For those skilled in the art, any obvious replacements that do not depart from the concept of the present invention are within the protection scope of the present invention.
Claims
1. An optical pressure-sensitive adhesive resistant to high temperature and humidity, characterized in that: The invention comprises component A and component B, wherein the component A comprises the following raw materials in parts by weight: 80-90 parts of acrylate monomer, 0.1-5 parts of functional monomer, 0.2-0.5 parts of initiator, 1-10 parts of silane coupling agent, 100-120 parts of solvent and 1-4 parts of auxiliary agent; the component B comprises the following raw materials in parts by weight: 1-3 parts of crosslinking agent and 1-2.5 parts of curing accelerator.
2. The high temperature and high humidity resistant optical pressure sensitive adhesive according to claim 1, characterized in that: The acrylic acid ester monomers are composed of methyl acrylate, butyl acrylate and aromatic ring-containing (meth) alkyl acrylate in a weight ratio of 1:5-10:2-5.
3. The high temperature and high humidity resistant optical pressure sensitive adhesive according to claim 2, characterized in that: The aromatic ring-containing alkyl (meth)acrylate is at least one of phenoxyethyl acrylate, benzyl acrylate, phenoxydiethylene glycol acrylate, phenoxyethyl methacrylate and benzyl methacrylate.
4. The high temperature and high humidity resistant optical pressure sensitive adhesive according to claim 2, characterized in that: The functional monomer is at least one of acrylic acid, hydroxyethyl acrylate, hydroxybutyl acrylate, methacrylic acid, hydroxyethyl acrylate, hydroxybutyl methacrylate and diacetone acrylamide.
5. The high temperature and high humidity resistant optical pressure sensitive adhesive according to claim 2, characterized in that: The functional monomer is composed of acrylic acid, hydroxyethyl acrylate and diacetone acrylamide in a weight ratio of 1:1-3:0.2-0.
5.
6. The high temperature and high humidity resistant optical pressure sensitive adhesive according to claim 1, characterized in that: The initiator is at least one of a peroxide initiator and an azo initiator.
7. The high temperature and high humidity resistant optical pressure sensitive adhesive according to claim 1, characterized in that: Each part of the auxiliary agent comprises the following raw materials in parts by weight: 0.5-2 parts of antioxidant and 0.5-2 parts of defoaming agent.
8. The method for preparing the high temperature and high humidity resistant optical pressure sensitive adhesive according to any one of claims 1 to 7, characterized in that: The steps include: (1) preparing component A and component B respectively; The preparation method of the A component comprises the following steps: (A1) adding part of the solvent to a reaction vessel, stirring and heating to 68-82° C., maintaining the temperature for 20-40 min and removing oxygen from the reaction vessel; (A2) mixing methyl acrylate, butyl acrylate, aromatic ring-containing alkyl (meth)acrylate, diacetone acrylamide and an initiator to obtain a mixture I; (A3) adding part of the mixture I to a reaction vessel, mixing evenly with the solvent treated in step (A1), controlling the temperature at 68-82° C., and reacting for 30-60 min; (A4) mixing hydroxyethyl acrylate, the remaining mixture I, a silane coupling agent and part of the solvent to obtain a mixture II; dropping the mixture II into a reaction vessel, keeping the temperature at 68-82° C., and completing the dropping within 250-210 min, and dropping part of the solvent; (A5) After the mixture II is added dropwise, the mixture is kept warm for 180-240 minutes, and then the auxiliary agent and the remaining solvent are added, and the mixture is stirred evenly to obtain the reaction solution. The reaction solution is cooled to room temperature, and then component A is added; The preparation method of the B component comprises the following steps: The crosslinking agent and the curing accelerator are uniformly mixed according to the weight ratio to prepare component B; (2) Component A and component B are mixed evenly to obtain an optical pressure-sensitive adhesive resistant to high temperature and high humidity.
9. A polarizer protective film, characterized in that: It comprises a base film and a pressure-sensitive adhesive layer arranged on the surface of the base film, wherein the pressure-sensitive adhesive layer is made of the aging-resistant pressure-sensitive adhesive according to any one of claims 1 to 7.
10. The method for preparing a protective film according to claim 9, characterized in that: The method comprises the following steps: mixing component A and component B evenly, then coating the mixture on the surface of the base film, drying the mixture at 110-120° C. for 3-10 minutes, and then maintaining the mixture at 55-65° C. for 20-30 hours.