Heat-conducting wear-resistant lubricating oil and preparation method thereof
Through functionalization treatment and emulsification technology, silicon carbide and boron nitride are uniformly dispersed in the lubricant, solving the problem of insufficient thermal conductivity and wear resistance in high-temperature environments, and achieving efficient heat dissipation and wear reduction effects .
Patent Information
- Application Number
- CN202410912070.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-07-09
AI Technical Summary
Traditional lubricating oils lack thermal conductivity and wear resistance in high-temperature and high-load environments, and silicon carbide and boron nitride powders have poor dispersion and insufficient stability in oil, which affects lubricating performance.
By functionalizing the silicon carbide and boron nitride, ball milling and emulsifying with kohlic acid and silane coupling agent, it is uniformly dispersed in the lubricating oil, combined with high-speed shear and centrifugal technology to ensure the stability and dispersion of the powder. .
It significantly improves the thermal conductivity and wear resistance of lubricating oil, maintains the viscosity and flowability of lubricating oil, and ensures the stable operation and long life of mechanical equipment under high temperature environments.
Smart Images

Figure HDA0004933927470000011
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of lubricating oils, and in particular to a heat-conducting and wear-resistant lubricating oil and a preparation method thereof. Background Art
[0002] Lubricants play a key role in the operation of mechanical equipment. Their main functions are to reduce friction, wear and dissipate heat. However, the performance of traditional lubricants in high temperature and high load environments is often unsatisfactory, mainly due to their insufficient thermal conductivity and wear resistance. As modern industry's requirements for equipment performance and reliability continue to increase, the development of lubricants with high thermal conductivity and high wear resistance has become a research hotspot.
[0003] Silicon carbide (SiC) and boron nitride (BN) are two materials that excel in thermal conductivity and wear resistance. Silicon carbide has high hardness, high thermal conductivity and good chemical stability, and is widely used in high temperature and wear resistant materials. Boron nitride, especially hexagonal boron nitride (h-BN), is known for its high thermal conductivity and lubricity and is called "white graphite". However, there are several problems with directly adding silicon carbide and boron nitride powders to lubricating oil:
[0004] Poor dispersibility: Silicon carbide and boron nitride powders tend to agglomerate in the oil phase and are difficult to disperse evenly, which affects the performance of the lubricating oil.
[0005] Insufficient stability: Untreated powder has poor stability in lubricating oil and is easy to settle, resulting in unstable lubricating oil performance.
[0006] Lubrication performance is affected: Directly adding powder may change the viscosity and fluidity of the lubricating oil, affecting its original lubrication performance. Summary of the invention
[0007] In order to solve the above problems, the present invention provides a heat-conducting and wear-resistant lubricating oil and a preparation method thereof.
[0008] In a first aspect, the present invention provides a method for preparing a heat-conducting and wear-resistant lubricating oil, wherein silicon carbide and boron nitride are functionalized by kojic acid, thereby improving the thermal conductivity and wear resistance thereof without affecting the lubrication effect. The components thereof are calculated by mass:
[0009] 85-95 parts of base oil, 0.5-2 parts of detergent, 0.1-1 parts of antioxidant, 0.5-2 parts of dispersant, 0.2-0.9 parts of passivator, 0.2-1 parts of rust inhibitor, 1-3 parts of functionalized silicon carbide and boron nitride mixed powder. The specific preparation method is as follows:
[0010] Step 1, silicon carbide and boron nitride powders are ball-milled in a mass ratio of 1: (0.5-2), the ball-milling medium is methanol, and a ball-milling liquid is obtained, and then kojic acid and a silane coupling agent are added to the ball-milling liquid in a mass ratio of 1: (3-10), and the total mass of kojic acid and the silane coupling agent is 2-10% of the ball-milling liquid, and then sheared and emulsified in a high-speed shearing machine;
[0011] Step 2, centrifuging the sheared emulsion to obtain a precipitate, adding deionized water to the precipitate, and then boiling it until a crystal precipitate is formed, grinding the precipitate and passing it through a 1000-3000 mesh sieve;
[0012] Step three, heating the base oil to 70-90 degrees, then adding detergent, antioxidant, dispersant, passivator, rust inhibitor and sieved precipitate according to mass proportion, stirring and mixing to obtain heat-conducting lubricating oil.
[0013] Preferably, in step 1, the silane coupling agent is one or more of KH550, KH560, and KH570, the ball milling rate is 200 to 800 rpm, and the total high-speed shearing time is 8 to 12 hours, wherein the shearing is paused for 5 minutes after every 30 to 60 minutes of shearing.
[0014] Preferably, in step 2, the centrifugal speed is 3500-7200 rcf, the centrifugal time is 30-90 min, and the mass of deionized water added is 50-100 times that of the precipitate.
[0015] Preferably, in step three, the stirring rate is 200-600 rpm, and the stirring time is 0.5-4 h.
[0016] In a second aspect, the present invention provides a heat-conducting and wear-resistant lubricating oil prepared by the preparation method of the first aspect of the present invention.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] 1. The functionalized silicon carbide and boron nitride of the present invention are uniformly dispersed in the lubricating oil, which significantly improves the thermal conductivity of the lubricating oil, can effectively dissipate heat, and maintain the stable operation of mechanical equipment in a high temperature environment.
[0019] 2. The high hardness characteristics of silicon carbide and boron nitride in the present invention give the lubricating oil excellent wear resistance, effectively reducing the wear between mechanical parts and extending the service life of the equipment.
[0020] 3. The functionalization treatment in the present invention ensures the uniform dispersion of silicon carbide and boron nitride powders in the lubricating oil, does not affect the viscosity and fluidity of the lubricating oil, and maintains the good lubricating effect of the lubricating oil. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions of the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0022] Figure 1 This is a comparison chart of the thermal conductivity of the lubricating oils prepared in the embodiments of the present invention and the comparative examples. DETAILED DESCRIPTION
[0023] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] Embodiment 1:
[0025] A heat-conducting wear-resistant lubricating oil and a preparation method thereof, wherein the components thereof are as follows by mass:
[0026] Base oil: 90 parts, detergent: 1.5 parts, antioxidant: 0.5 parts, dispersant: 1.5 parts, passivator: 0.5 parts, rust inhibitor: 0.5 parts, functionalized silicon carbide and boron nitride mixed powder: 2 parts
[0027] The preparation method is as follows:
[0028] Silicon carbide and boron nitride powders were mixed by ball milling at a mass ratio of 1:1, with methanol as the ball milling medium, to obtain a ball milling solution. Kojic acid and silane coupling agent KH550 were added, with a mass ratio of 1:5 and a total mass of 5% of the ball milling solution. The mixture was then sheared at 600 rpm for 10 hours in a high-speed shearing machine, with a 5-minute pause after every 30 minutes of shearing.
[0029] The sheared emulsion was centrifuged at 5000 rcf for 60 minutes to obtain a precipitate. The precipitate was added with deionized water, 75 times the mass of the precipitate, and then boiled to form a crystal precipitate. The precipitate was ground and passed through a 2000 mesh sieve.
[0030] The base oil was heated to 80 degrees, and then detergent, antioxidant, dispersant, passivator, rust inhibitor and sieved precipitate were added according to mass proportions, the stirring rate was 400 rpm, and the stirring time was 2 hours to obtain thermal conductive lubricating oil.
[0031] Embodiment 2:
[0032] A heat-conducting wear-resistant lubricating oil and a preparation method thereof, wherein the components thereof are as follows by mass:
[0033] Base oil: 85 parts, detergent: 1 part, antioxidant: 0.8 parts, dispersant: 1.2 parts, passivator: 0.7 parts, rust inhibitor: 0.8 parts, functionalized silicon carbide and boron nitride mixed powder: 1.5 parts
[0034] The preparation method is as follows:
[0035] Silicon carbide and boron nitride powders were mixed by ball milling at a mass ratio of 1:1.5, with methanol as the ball milling medium, to obtain a ball milling solution. Kojic acid and silane coupling agent KH560 were added, with a mass ratio of 1:7 and a total mass of 8% of the ball milling solution. The mixture was then sheared at 500 rpm for 8 hours in a high-speed shearing machine, with a 5-minute pause after every 45 minutes of shearing.
[0036] The sheared emulsion was centrifuged at 6000 rcf for 45 minutes to obtain a precipitate. The precipitate was added with deionized water 60 times the mass of the precipitate and then boiled until a crystal precipitate formed. The precipitate was ground and passed through a 1500 mesh sieve.
[0037] The base oil was heated to 75 degrees, and then detergent, antioxidant, dispersant, passivator, rust inhibitor and sieved precipitate were added according to mass proportions, the stirring rate was 300 rpm, and the stirring time was 1 hour to obtain a thermal conductive lubricating oil.
[0038] Embodiment 3:
[0039] A heat-conducting wear-resistant lubricating oil and a preparation method thereof, wherein the components thereof are as follows by mass:
[0040] Base oil: 95 parts, detergent: 0.5 parts, antioxidant: 0.2 parts, dispersant: 0.8 parts, passivator: 0.3 parts, rust inhibitor: 0.3 parts, functionalized silicon carbide and boron nitride mixed powder: 3 parts
[0041] The preparation method is as follows:
[0042] Silicon carbide and boron nitride powders were mixed by ball milling at a mass ratio of 1:2, with methanol as the ball milling medium, to obtain a ball milling solution. Kojic acid and silane coupling agent KH570 were added, with a mass ratio of 1:3 and a total mass of 10% of the ball milling solution. The mixture was then sheared at 400 rpm for 12 hours in a high-speed shearing machine, with a 5-minute pause after every 60 minutes of shearing.
[0043] The sheared emulsion was centrifuged at 7200 rcf for 90 minutes to obtain a precipitate. The precipitate was added with deionized water 100 times the mass of the precipitate, and then boiled until a crystal precipitate formed. The precipitate was ground and passed through a 3000 mesh sieve.
[0044] The base oil was heated to 90 degrees, and then detergent, antioxidant, dispersant, passivator, rust inhibitor and sieved precipitate were added according to mass proportions, the stirring rate was 600 rpm, the stirring time was 4 hours, and the thermal conductive lubricating oil was obtained.
[0045] Comparative Example:
[0046] A heat-conducting wear-resistant lubricating oil and a preparation method thereof, wherein the components thereof are as follows by mass:
[0047] Base oil: 90 parts, detergent: 1.5 parts, antioxidant: 0.5 parts, dispersant: 1.5 parts, passivator: 0.5 parts, rust inhibitor: 0.5 parts, unfunctionalized silicon carbide and boron nitride mixed powder: 2 parts
[0048] The preparation method is as follows:
[0049] Silicon carbide and boron nitride powders were mixed by ball milling at a mass ratio of 1:1, with methanol as the ball milling medium, to obtain a ball milling solution. Silane coupling agent KH550 was added, with a total mass of 5% of the ball milling solution. Then, the mixture was sheared at 600 rpm for 10 hours in a high-speed shearing machine, and the mixture was paused for 5 minutes after every 30 minutes of shearing.
[0050] The sheared emulsion was centrifuged at 5000 rcf for 60 minutes to obtain a precipitate. The precipitate was added with deionized water, 75 times the mass of the precipitate, and then boiled to form a crystal precipitate. The precipitate was ground and passed through a 2000 mesh sieve.
[0051] The base oil was heated to 80 degrees, and then detergent, antioxidant, dispersant, passivator, rust inhibitor and sieved precipitate were added according to mass proportions, the stirring rate was 400 rpm, and the stirring time was 2 hours to obtain thermal conductive lubricating oil.
Claims
1. A method for preparing a heat-conducting and wear-resistant lubricating oil, characterized in that: Kojic acid is used to functionalize silicon carbide and boron nitride, thereby improving their thermal conductivity and wear resistance without affecting the lubrication effect. The components are calculated by mass: 85-95 parts of base oil, 0.5-2 parts of detergent, 0.1-1 parts of antioxidant, 0.5-2 parts of dispersant, 0.2-0.9 parts of passivator, 0.2-1 parts of rust inhibitor, 1-3 parts of functionalized silicon carbide and boron nitride mixed powder. The specific preparation method is as follows: Step 1, silicon carbide and boron nitride powders are ball-milled in a mass ratio of 1: (0.5-2), the ball-milling medium is methanol, and a ball-milling liquid is obtained, and then kojic acid and a silane coupling agent are added to the ball-milling liquid in a mass ratio of 1: (3-10), and the total mass of kojic acid and the silane coupling agent is 2-10% of the ball-milling liquid, and then sheared and emulsified in a high-speed shearing machine; Step 2, centrifuging the sheared emulsion to obtain a precipitate, adding deionized water to the precipitate, and then boiling it until a crystal precipitate is formed, grinding the precipitate and passing it through a 1000-3000 mesh sieve; Step three, heating the base oil to 70-90 degrees, then adding detergent, antioxidant, dispersant, passivator, rust inhibitor and sieved precipitate according to weight proportion, stirring and mixing to obtain heat-conducting lubricating oil.
2. The method for preparing heat-conducting and wear-resistant lubricating oil according to claim 1, characterized in that: In step 1, the silane coupling agent is one or more of KH550, KH560, and KH570, the ball milling rate is 200 to 800 rpm, and the total high-speed shearing time is 8 to 12 hours, wherein the shearing is paused for 5 minutes after every 30 to 60 minutes of shearing.
3. The method for preparing a conductive-insulating double-layer glass coating according to claim 1, characterized in that: In step 2, the centrifugal speed is 3500-7200 rcf, the centrifugal time is 30-90 min, and the mass of deionized water added is 50-100 times that of the precipitate.
4. The method for preparing a conductive-insulating double-layer glass coating according to claim 1, characterized in that: In step 3, the stirring rate is 200-600 rpm, and the stirring time is 0.5-4 h.
5. A heat-conducting, wear-resistant lubricating oil prepared by the preparation method according to any one of claims 1 to 4.
Citation Information
Patent Citations
Insulating heat-conducting lubricating oil and preparation method thereof
CN117801868A
Method for preparing nanocomposite material for toe cap production
US20230235154A1
High-performance lubricant oil
US5985802A
Highly insulating silicon carbide / boron nitride ceramic material and preparation method therefor