Optimization process for preparing CuSn10 alloy through selective laser melting

Through the selection laser melting technology and response surface method optimization process parameters, the density and performance problems of high-tin bronze parts in traditional casting processes are solved, and the preparation of CuSn10 alloy with high density and excellent mechanical properties is achieved, reducing costs and expanding processing route.

CN118979170APending Publication Date: 2024-11-19SHENYANG UNIVERSITY OF TECHNOLOGY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411096148.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The high-tin bronze parts produced by traditional casting processes have defects such as low density, shrinkage, microcracks, and severe segregation, resulting in poor performance and high cost.

Method used

Selected laser melting technology is used to print CuSn10 alloy powder layer by layer through Z-shaped scanning, and optimize process parameters in combination with the response surface method to achieve alloy preparation with high density and excellent mechanical properties.

Benefits of technology

The high density and excellent mechanical properties of CuSn10 alloy are achieved, which reduces costs and expands the processing and preparation route of the alloy, avoiding defects and high cost problems in traditional processes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979170A_ABST
    Figure CN118979170A_ABST
Patent Text Reader

Abstract

The invention discloses an optimization process for preparing CuSn10 alloy through selective laser melting, which is characterized in that the defects such as air holes and cracks in a formed part are reduced by adjusting process parameters in a laser printing process, such as laser power, scanning speed and powder layer thickness, so that the density of the formed part is improved, and the quality of the formed part is improved. And finally, the performance of the CuSn10 alloy part is improved. In addition, due to the characteristic of rapid solidification of selective laser melting, a finer microstructure can be obtained. The prepared CuSn10 alloy has excellent mechanical properties while achieving high density.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of energy utilization, and in particular to an optimized process for preparing CuSn10 alloy by selective laser melting. Background Art

[0002] Tin bronze mainly includes copper and tin elements. It is one of the oldest traditional alloys known to mankind, so its application field is also very wide. Generally speaking, tin bronze can be used for plastic processing and is widely used in the electrical and electronic industries, such as sensitive components of pressure gauges and electrical connectors, as well as high-precision electrical connectors and sensitive components such as high-precision springs. With the increase of tin content, the mechanical properties of tin bronze can be enhanced. High-tin bronze has excellent mechanical properties, wear resistance and corrosion resistance, so it can be used in the navigation and mechanical industries, such as ship parts and bearings. The main manufacturing technology for high-tin bronze is casting. High-tin bronze parts produced by traditional casting processes have a large number of defects, such as low density, shrinkage cavities and microcracks, severe segregation and other defects.

[0003] Therefore, the prior art still needs to be improved and enhanced. Summary of the invention

[0004] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide an optimized process for preparing CuSn10 alloy by selective laser melting, aiming to solve the problems of low density, shrinkage cavities and microcracks, severe segregation and other defects of high-tin bronze parts produced by traditional casting processes.

[0005] In order to achieve the above object, the present invention adopts the following technical solutions: In a first aspect, an optimized process for preparing CuSn10 alloy by selective laser melting comprises the following steps: Step 1: Weigh the CuSn10 alloy powder and pretreat it, the chemical composition of the powder is Sn element is 10.02wt.%, and the rest is Cu element; Step 2: Fill the top powder chamber with alloy powder and lay the alloy powder on the substrate, then use inert gas to purge the printing chamber until the oxygen content in the chamber is less than 10ppm; Step 3: The laser of the selective laser melting equipment prints the alloy powder layer by layer according to the set process file; the laser of the printing equipment adopts a Z-shaped scanning method, and the rotation angle of the laser scanning direction of adjacent processing layers is 90°; Step 4: Use different process parameters for printing, use response surface methodology to optimize the density, complete printing, and obtain a high-density alloy.

[0006] Furthermore, in step 1, the pretreatment is a drying treatment of the powder, and the oven temperature during the drying treatment is 100-120° C. and the time is 4-8 hours.

[0007] Furthermore, in step 2, the thickness of the laid alloy powder is 20-30 μm, and the height of the alloy powder in the top powder chamber is 2-3 times the height of the prepared CuSn10 alloy.

[0008] Further, in step 3, the steps of printing layer by layer are: The laser spot of the printing device laser scans on the printing substrate in a zigzag scanning manner, sintering and melting the alloy powder pre-laid on the substrate and rapidly cooling and solidifying it into a prepared plane, completing the first printing; The alloy powder is laid again on the prepared plane of the substrate using a hook, and then the height of the substrate is lowered, and the laser path of the laser is rotated to sinter the alloy powder on the prepared plane in a Z-shaped scanning manner within the layer to complete the second printing; Repeat step three in sequence until a CuSn10 alloy block is obtained.

[0009] Furthermore, in step 4, the thickness of the laid powder is 20-30 μm, the laser power is 215-275 W, the scanning speed is 600-900 mm / s, and the scanning interval is fixed at 100 μm.

[0010] Furthermore, in step 4, the response surface experimental method was adopted, and the experimental results were analyzed using Design Expert; laser power, scanning speed and powder layer thickness were used as design variables, and density was used as the objective function; high, medium and low levels of different factors were represented by +1, 0 and -1, respectively.

[0011] Furthermore, in step 4, the response surface methodology used a response surface experiment with three factors and three levels, designed a total of 17 groups of experiments, and printed and formed the 17 groups of specimens respectively.

[0012] Furthermore, the response surface experiment method is adopted and the test results are analyzed by using Design Expert, including: Through reasonable experimental design methods and the obtained experimental data, the functional relationship between factors and response values ​​is fitted using multivariate quadratic regression equations, and statistical analysis is performed on them; Considering the interaction between various factors, a high-order polynomial is selected, and the approximate function selects the general second-order density model to perform variance analysis on the processing parameters; the model can be expressed as follows: ; Among them, y is the response value, that is, the density in this study; X is the design variable, β0 represents a constant, and β i , β ij , β iiare the coefficients of linear effect, interaction effect and quadratic effect respectively, i, j, k are constant coefficients, and 𝜀 is the random error.

[0013] The technical solution adopted by the present invention has the following beneficial effects: In the present invention, a selective laser melting optimization process for preparing CuSn10 alloy can obtain a more refined microstructure by using the rapid solidification characteristics of the selective laser melting technology. Through the selective laser melting technology, in the process of building the model layer by layer, the larger temperature gradient between the molten pool and the substrate will make the solidification process faster, so that the grain size of the alloy is smaller and the comprehensive performance is better. At the same time, dislocations can be introduced by the Z-shaped scanning method, so that the strength of the CuSn10 alloy can be improved, and good room temperature processing performance can be maintained. More precise and complex parts can be prepared. At the same time, the use of powder recovery can also effectively reduce costs, solving the high cost problem existing in the prior art. Finally, through the response surface method, multiple groups of experiments are designed, and the functional relationship between the multivariate quadratic regression equation fitting factors and the response value is used to search for the optimal process parameters, and the multivariate problem is solved by analyzing the regression equation to obtain the optimal process parameters for selective laser melting printing of CuSn10 alloy. The preparation of CuSn10 alloy with high density and excellent mechanical properties is achieved, and the processing and preparation route of the alloy is expanded. BRIEF DESCRIPTION OF THE DRAWINGS

[0014] Figure 1 This is a flow chart of preparing CuSn10 alloy by laser melting in an embodiment of the present invention; Figure 2 The surface morphology diagram of the optimal process parameters for laser melting selected in the embodiment of the present invention; Figure 3 A metallographic defect diagram showing the best process parameters for laser melting selected in an embodiment of the present invention; Figure 4 The melt width morphology diagram of the optimal process parameters for laser melting selected in the embodiment of the present invention; Figure 5 The cross-sectional morphology of the molten pool is selected for the optimal laser melting process parameters in the embodiment of the present invention; Figure 6 It is a fitting diagram of density prediction value and test value of response surface method in an embodiment of the present invention; Figure 7 It is a contour map and a 3D-RSM map of the two-factor interaction of the response surface method in an embodiment of the present invention. DETAILED DESCRIPTION

[0015] In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail with reference to the accompanying drawings and examples. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0016] The present invention discloses an optimized process for preparing CuSn10 alloy by selective laser melting. Figure 1 , including the following steps: Step 1: Weigh a sufficient amount of CuSn10 powder, the composition of which is calculated by mass percentage, with the mass percentage of Sn element being 10.02% and the rest being Cu element.

[0017] Before the experiment, put the CuSn10 powder into an oven (100-120°C) and dry it for 4-8 hours. Prepare 316 stainless steel sheet as the printing substrate.

[0018] Step 2: Use anhydrous ethanol with a concentration greater than 99% to clean the printing chamber, fill the alloy powder into the top powder chamber, and then pass inert gas (argon) to purge the equipment until the oxygen content in the chamber is less than 10ppm.

[0019] Step 3: The laser spot of the equipment uses a Z-shaped scanning method to print the alloy powder layer by layer.

[0020] Among them, the printing method is to use 3D modeling software to process the model file in .stl format, use slicing software to set the process parameters and export it as a working file in .ojob format, and finally import it into the device for printing.

[0021] The specific steps for obtaining the CuSn10 alloy bulk are: The laser spot scans the laid alloy powder layer by layer in a strip manner, sintering and melting the alloy powder and quickly cooling it to form a prepared plane, completing the first layer of printing.

[0022] Alloy powder (thickness 20-30μm) is laid on the prepared plane formed by the first layer of printing, and then the printed substrate is lowered (the lowering height is the thickness of the powder layer), the laser scanning path of the laser is rotated (the angle is 90°), and the laser spot scans the laid alloy powder layer by layer in a strip manner again to complete the second layer of printing.

[0023] Repeat the printing method for the second layer. The laser of the selective laser melting equipment prints the alloy powder according to the pre-designed process. After each layer is printed, the substrate drops to a fixed height. The scraper evenly spreads the alloy powder in the top powder chamber on the printed preparation plane and performs laser scanning again. The cycle is repeated in sequence to achieve efficient bonding within and between layers through rapid melting and cooling solidification until a CuSn10 alloy block is obtained.

[0024] Step 4: Use the response surface experimental method and use Design Expert to analyze the test results. According to the BBD (Box-Behnken) principle, laser power (A), scanning speed (B) and powder layer thickness (C) are used as design variables, and density (Y) is the objective function. The high, medium and low levels of different factors are represented by +1, 0 and -1 respectively. A response surface experiment with 3 factors and 3 levels was designed. A total of 17 groups of experiments were designed and these 17 specimens were printed according to the above method.

[0025] Through reasonable experimental design methods and the obtained experimental data, the functional relationship between factors and response values ​​is fitted with multivariate quadratic regression equations, and statistical analysis is performed on them.

[0026] Considering the interaction between various factors, a high-order polynomial is selected, and the approximate function can select a general second-order density model to perform variance analysis on the processing parameters. The model can be expressed as follows: Among them, y is the response value, that is, the density in this study. β0 represents a constant, β i , β ij , β ii are the coefficients of linear effect, interaction effect and quadratic effect respectively, and 𝜀 is the random error.

[0027] The functional relationship between factors and response values ​​is fitted by multivariate quadratic regression equations to search for optimal process parameters, and multivariate problems are solved by analyzing regression equations.

[0028] Finally, the significance and suitability of the quadratic regression model and the significant effect of the interaction on the response value (density) were determined by variance analysis.

[0029] In ANOVA, the F value is used to test the hypothesis that "the means of all treatments are equal". Then, the F value is calculated and compared with the standard value. The P value represents the probability that the calculated F value is greater than the standard value, indicating the significance level of the influencing factor. Traditionally, it is stipulated that a P value less than 0.05 indicates statistical significance, and less than 0.01 indicates highly significant.

[0030] After printing is completed, wait for the equipment to cool naturally to room temperature, then remove the printed substrate and the specimen on the substrate, and separate the specimen from the substrate by wire cutting. Add anhydrous ethanol to the ultrasonic cleaner to clean the specimen for 20 minutes, then take it out and air dry it. Then use the Archimedes drainage method to test the density of the specimen. Next, inlay the specimen, polish it with 200#, 400#, 600#, 1000#, 1500#, and 2000# sandpaper, polish it on the damping cloth with alumina polishing liquid and diamond polishing paste, clean it and blow it dry.

[0031] The specimens were observed through an ultra-depth-of-field microscope to observe and compare the surface morphology and metallographic defects (holes, cracks) of different specimens.

[0032] The Z-shaped scanning method has a small laser span, which greatly reduces the processing time and improves the processing efficiency.

[0033] Rotating the laser scanning direction by 90° between adjacent processing layers helps to achieve more uniform melting of the powder spreading area, effectively avoids defects such as deformation, delamination and cracks in the processed parts, and improves the mechanical properties of the processed specimens.

[0034] The thickness of the laid alloy powder is 20~30μm, mainly because the laser absorption rate of Cu alloy powder is low. The moderate powder thickness can help the absorption of powder laser and reduce production costs.

[0035] The height of the alloy powder in the top powder chamber is 2 to 3 times the height of the prepared CuSn10 alloy. This helps the scraper to evenly spread the alloy powder in the top powder chamber on the processing plane and reduce the occurrence of defects during the processing.

[0036] The present invention uses a selective laser melting method to prepare the CuSn10 alloy. This processing method has the characteristics of rapid melting and solidification, so a more refined organizational microstructure can be obtained, the grain size of the alloy will also be smaller, and the comprehensive performance will be significantly improved.

[0037] Among them, the Z-shaped scanning method has a small laser span, which greatly reduces the processing time and improves the processing efficiency.

[0038] Rotating the laser scanning direction by 90° between adjacent processing layers helps to achieve more uniform melting of the powder spreading area, effectively avoids defects such as deformation, delamination and cracks in the processed parts, and improves the mechanical properties of the processed specimens.

[0039] The thickness of the laid alloy powder is 20~30μm, mainly because the laser absorption rate of Cu alloy powder is low. The moderate powder thickness can help the absorption of powder laser and reduce production costs.

[0040] The height of the alloy powder in the top powder chamber is 2 to 3 times the height of the prepared CuSn10 alloy. This helps the scraper to evenly spread the alloy powder in the top powder chamber on the processing plane and reduce the occurrence of defects during the processing.

[0041] Finally, the response surface method is used to transform complex multivariate relationships into simple two-dimensional or three-dimensional graphs, so that the relationship between various processing parameters and other variables in selective laser melting can be understood more intuitively, and the optimal processing parameters can be obtained with fewer trials, thereby improving efficiency and reducing costs.

[0042] Example 1.

[0043] Step 1: Weigh enough CuSn10 powder. Before the experiment, put the CuSn10 powder into an oven (100-120°C) and dry it for 4-8 hours. Prepare 316 stainless steel sheet as the printing substrate.

[0044] Step 2: Use anhydrous ethanol with a concentration greater than 99% to clean the printing chamber, fill the powder into the top powder chamber, and then pass inert gas (argon) to purge the equipment until the oxygen content in the chamber is below 10ppm.

[0045] Step 3: The laser of the selective laser melting equipment prints the alloy powder according to the set process file. After each layer of printing is completed, the substrate drops to a fixed height (layer thickness), and the scraper evenly spreads the alloy powder in the top powder chamber on the prepared plane to complete the second layer of printing. The process is repeated in sequence, and efficient bonding within and between layers is achieved through rapid melting and cooling solidification until a CuSn10 alloy block is obtained. Among them, the laser power is 215W, 245W, and 275W, the scanning speed is 600mm / s, 750mm / s, and 900mm / s, the powder layer thickness is fixed at 20μm, and the scanning spacing is fixed at 100μm.

[0046] After printing is completed, wait for the equipment to cool naturally to room temperature, then remove the printed substrate and the specimen on the substrate, and separate the specimen from the substrate by wire cutting. Add anhydrous ethanol to the ultrasonic cleaner to clean the specimen for 20 minutes, then take it out and air dry it. Then use the Archimedes drainage method to test the density of the specimen. Next, inlay the specimen, polish it with 200#, 400#, 600#, 1000#, 1500#, and 2000# sandpaper, polish it on the damping cloth with alumina polishing liquid and diamond polishing paste, clean it and blow it dry.

[0047] The specimens were observed through an ultra-depth-of-field microscope to observe and compare the surface morphology and metallographic defects (holes, cracks) of different specimens.

[0048] Example 2.

[0049] The difference from Example 1 is that the laser power is 215 W, 245 W, and 275 W, the scanning speed is 600 mm / s, 750 mm / s, and 900 mm / s, the powder layer thickness is fixed at 25 μm, and the scanning interval is fixed at 100 μm.

[0050] Example 3.

[0051] The difference from Example 1 is that the laser power is 215 W, 245 W, and 275 W, the scanning speed is 600 mm / s, 750 mm / s, and 900 mm / s, the powder layer thickness is fixed at 30 μm, and the scanning interval is fixed at 100 μm.

[0052] Example 4.

[0053] The density of various specimens in Example 1, Example 2, and Example 3 is summarized. The test results are analyzed using Design Expert. Laser power (A), scanning speed (B), and powder layer thickness (C) are set as design variables, and density (Y) is the objective function. The high, medium, and low levels of different factors are represented by +1, 0, and -1, respectively. The response surface method factors and level designs of these 17 groups of specimens are shown in Table 1.

[0054] Table 1 Box-Behnken factor and level design Through reasonable experimental design methods and the obtained experimental data, the functional relationship between the factors and the response values ​​was fitted using the multivariate quadratic regression equation, and statistical analysis was performed. Table 2 shows the relative density of the specimens under different processing parameter settings.

[0055] Table 2 Response surface experiment results The significance and suitability of the quadratic regression model and the significant effect of the interaction on the response value (density) were determined by analysis of variance. The F value was used to test the assumption that "the means of all treatments are equal". Then, the F value was calculated and compared with the standard value. The probability that the F value calculated by the P value is greater than the standard value indicates the significance level of the influencing factor. Traditionally, it is stipulated that a P value less than 0.05 indicates statistical significance, and less than 0.01 indicates high significance. Table 3 shows the results of the analysis of variance of the response surface.

[0056] Table 3 Analysis of variance of regression equation In order to obtain a suitable model, the accuracy test was carried out. Based on the fitting results, the accuracy of the mathematical model related to density was tested by combining residual analysis and data point distribution law. The fitting diagram of the predicted value and the tested value of the density of CuSn10 specimen is shown in Figure 2. Figure 6 As shown in Figure 2, the model prediction values ​​and actual values ​​are distributed with high density on both sides of the straight line, and the density on both sides of the straight line is very small. Figure 5 The points in are roughly distributed on a straight line, which further proves that the above fitting results meet the actual requirements and the obtained mathematical model has high reliability.

[0057] The response surface plot can more intuitively reflect the impact of two-factor interaction on the response. Figure 7The contour map and 3D-RSM map of the two-factor interaction show the interactive effects of laser power, scanning speed and powder layer thickness on the density of the specimen, and clearly show the peak value of density. The optimal density prediction value can reach 99.82%, and the corresponding processing parameters are laser power 247W, scanning speed 785mm / s, and powder layer thickness 0.2mm.

[0058] The surface morphology of the specimen under the optimal parameters is as follows Figure 2 As shown in the figure, the common flaky features in SLM can be observed, with a clear and uniform molten pool morphology and a smooth surface, without the generation of obvious defects (cracks, holes), which further illustrates the goodness of the optimized parameters. Figure 3 This is the metallographic image obtained after the specimen was ground and polished. It can be seen that there are no cracks on the specimen, only a small amount of micro pores. Figure 4 This is a microscopic melt path diagram under the optimal parameters. From the figure, we can see the evenly distributed long strips of melt paths, which is mainly because the specimen is formed by the overlap of many melt paths during the scanning process of the laser heat source. The width and length of each melt path are also different, which is mainly due to the uneven distribution of metal powder particles and the accumulation of temperature during the scanning process of the laser heat source, which leads to different surface tensions of the melt paths. Figure 5 This is the cross-sectional morphology of the molten pool obtained by etching the side of the specimen. It can be clearly seen that the cross-sectional appearance of the specimen shows a unique fish-scale structure. This morphology helps to closely combine different scanning layers. After measurement, the depth of the molten pool is higher than the thickness of the powder layer.

[0059] CuSn10 specimens with different process parameters (laser power, scanning speed, powder layer thickness) were prepared by Example 1, Example 2, and Example 3. Response surface methodology was used by Example 4, using a reasonable experimental design method and the obtained experimental data, and the functional relationship between the multivariate quadratic regression equation was used to fit the factor and the response value, and statistical analysis was performed on it. The optimal process parameters were searched by fitting the functional relationship between the factor and the response value by the multivariate quadratic regression equation.

[0060] It is found that the influence of laser power, scanning speed and powder layer thickness on the density of the specimen is not unique, and they all have a reasonable range of values. Laser power is an important indicator for determining the input energy in the SLM molding process, which directly determines the melting degree of the temperature field formed by the laser on the powder material. If the laser power is too low, the powder will not melt completely. If the laser power is too high, the powder may burn excessively.

[0061] Scanning speed indicates the distance the laser moves on the powder bed per unit time. It determines the ability of the powder to absorb laser energy per unit time. The energy absorption capacity of the powder per unit area is negatively correlated with the scanning speed, resulting in poor melt pool stability and easy balling. As the scanning speed increases, the energy input increases, the single channel morphology becomes more irregular, accompanied by non-uniformity of the single channel width and a higher balling rate.

[0062] Although the powder layer thickness has a relatively small impact on SLM printed parts, it is also an important parameter that affects the molding quality. By adjusting the powder layer thickness, good overlap between powder layers can be achieved to achieve efficient molding. A thicker powder layer thickness can significantly increase the printing rate, but unlimited increase in powder layer thickness can easily lead to an increase in the number and size of defects due to the increase in powder layer thickness, which is caused by the multiple reflections of the laser beam in the pores, thus seriously affecting the mechanical properties of the parts.

[0063] Those skilled in the art will readily appreciate other embodiments of the present invention after considering the specification and practicing the schemes disclosed herein. The present invention is intended to cover any variations, uses or adaptations of the present invention that follow the general principles of the present invention and include common knowledge or customary techniques in the art that are not disclosed in this disclosure. The description and examples are to be considered exemplary only, and the true scope and spirit of the present invention are indicated by the claims.

Claims

1. An optimized process for preparing CuSn10 alloy by selective laser melting, characterized in that: The following steps are involved: Step 1: Weigh the CuSn10 alloy powder and pretreat it, the chemical composition of the powder is Sn element is 10.02wt.%, and the rest is Cu element; Step 2: Fill the top powder chamber with alloy powder and lay the alloy powder on the substrate, then use inert gas to purge the printing chamber until the oxygen content in the chamber is less than 10ppm; Step 3: The laser of the selective laser melting equipment prints the alloy powder layer by layer according to the set process file; the laser of the printing equipment adopts a Z-shaped scanning method, and the rotation angle of the laser scanning direction of adjacent processing layers is 90°; Step 4: Use different process parameters for printing, use response surface methodology to optimize the density, complete printing, and obtain a high-density alloy.

2. The optimized process for preparing CuSn10 alloy by selective laser melting according to claim 1 is characterized in that: In step 1, the pretreatment is a drying treatment of the powder, and the oven temperature during the drying treatment is 100-120° C. and the time is 4-8 hours.

3. The optimized process for preparing CuSn10 alloy by selective laser melting according to claim 1 is characterized in that: In step 2, the thickness of the laid alloy powder is 20-30 μm, and the height of the alloy powder in the top powder chamber is 2-3 times the height of the prepared CuSn10 alloy.

4. The optimized process for preparing CuSn10 alloy by selective laser melting according to claim 1 is characterized in that: In step 3, the steps of printing layer by layer are: The laser spot of the printing device laser scans on the printing substrate in a zigzag scanning manner, sintering and melting the alloy powder pre-laid on the substrate and rapidly cooling and solidifying it into a prepared plane, completing the first printing; The alloy powder is laid again on the prepared plane of the substrate using a hook, and then the height of the substrate is lowered, and the laser path of the laser is rotated to sinter the alloy powder on the prepared plane in a Z-shaped scanning manner within the layer to complete the second printing; The above steps are repeated sequentially until a CuSn10 alloy block is obtained.

5. The optimized process for preparing CuSn10 alloy by selective laser melting according to claim 1, characterized in that: In step 4, the thickness of the laid powder is 20-30 μm, the laser power is 215-275 W, the scanning speed is 600-900 mm / s, and the scanning interval is fixed at 100 μm.

6. The optimized process for preparing CuSn10 alloy by selective laser melting according to claim 1, characterized in that: In step 4, the response surface method was used, and the experimental results were analyzed using Design Expert; laser power, scanning speed, and powder layer thickness were used as design variables, and density was used as the objective function; high, medium, and low levels of different factors were represented by +1, 0, and -1, respectively.

7. The optimized process for preparing CuSn10 alloy by selective laser melting according to claim 1, characterized in that: In step 4, the response surface methodology used a response surface experiment with three factors and three levels, designed a total of 17 groups of experiments, and printed and formed the 17 groups of specimens separately.

8. The optimized process for preparing CuSn10 alloy by selective laser melting according to claim 6 is characterized in that: The response surface experiment method is adopted and the test results are analyzed by using Design Expert, including: Through reasonable experimental design methods and the obtained experimental data, the functional relationship between factors and response values ​​is fitted using multivariate quadratic regression equations, and statistical analysis is performed on them; Considering the interaction between various factors, a high-order polynomial is selected, and the approximate function selects the general second-order density model to perform variance analysis on the processing parameters; the model can be expressed as follows: ; Among them, y is the response value, that is, the density in this study; X is the design variable, β0 represents a constant, and β i , β ij , β ii are the coefficients of linear effect, interaction effect and quadratic effect respectively, i, j, k are constant coefficients, and 𝜀 is the random error.

Citation Information

Cited By

  • A copper-based porous self-lubricating material and its preparation method