Equipment for preparing gallium arsenide single crystal and preparation method of gallium arsenide single crystal
By using a combination technology of magnets, boron oxide crucibles and nitrogen to maintain air pressure during GaAs single crystal growth, combined with ultrasonic vibration and vertical gradient condensation, the problems of chemical proportional ratio of GaAs single crystals and the introduction of impurities are solved, and high quality is achieved The single crystal preparation of gallium arsenide improves device performance.
Patent Information
- Application Number
- CN202411083684.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-19
AI Technical Summary
GaAs single crystals have chemical proportion imbalance problems during high-temperature growth, resulting in stress aggregation defects and affect device performance. The existing technology is difficult to effectively solve the problems of arsenic-rich phenomenon and the boron oxide layer absorbs water and decomposes B impurities.
Using equipment including a single crystal synthesis furnace, step-shaped quartz tube and ultrasonic flat plate, the magnetic field is generated by magnets, direct oxidation of boron oxide crucibles and nitrogen to maintain air pressure, combined with vertical gradient condensation method and ultrasonic vibration, the growth of gallium arsenide single crystal is controlled. The process reduces the introduction of B impurities and metal impurities, and improves chemical proportional balance and purity.
It significantly improves the crystal formation rate and internal purity of the single crystal of gallium arsenide, reduces the dislocation density defect, improves device performance, and achieves high-quality GaAs single crystal preparation.
Smart Images

Figure BDA0004984545390000091 
Figure HDA0004984545400000011 
Figure HDA0004984545400000012
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor technology, and in particular to a device for preparing a gallium arsenide single crystal and a method for preparing a gallium arsenide single crystal. Background Art
[0002] In recent years, the rapid development of mobile communications, network technology and the electronics industry has driven the development of the gallium arsenide (GaAs) industry. At present, GaAs single crystal materials have become an important basic material for microelectronics and optoelectronics, and have been widely used in the manufacture of microwave high-power devices, low-noise devices, microwave millimeter-wave monolithic integrated circuits, ultra-high-speed digital circuits and other electronic devices.
[0003] However, the growth process of GaAs single crystal is complicated, and there is a problem of chemical imbalance during the high-temperature growth process, which leads to stress accumulation defects in GaAs single crystals, and then makes its electrical parameters fail to meet the use requirements. The main reasons for the chemical imbalance problem are: 1) When growing GaAs single crystals, boron oxide is often needed as a sealant to prevent GaAs from decomposing at high temperatures or GaAs melt from directly contacting the inner wall of the boron nitride crucible to form twins, but boron oxide is generated by heating the boron nitride crucible through oxygen reaction. After the reaction, the boron nitride crucible is cooled to room temperature before loading. During the cooling process of the boron nitride crucible, since it is not a sealed environment, the boron oxide layer formed on the inner wall of the crucible easily absorbs moisture, and then decomposes B impurities. Therefore, the use of boron oxide introduces a large amount of B impurities. During the growth process of GaAs single crystals, B impurities occupy 1) The Ga position makes the chemical ratio of Ga low and arsenic-rich sites appear; 2) The metal impurity ions such as Fe, Ca, Al, Zn, Cu in GaAs will form metal compounds with As, Si, and O, further aggravating the imbalance of the chemical ratio of GaAs; 3) The growth of GaAs single crystal requires the addition of a small amount of elemental As in a sealed quartz tube, and the elemental As is used to form As vapor under high temperature to maintain the pressure balance in the quartz tube, avoiding the decomposition of GaAs or the compression and rupture of the quartz tube due to insufficient air pressure. However, the addition of elemental As often aggravates the arsenic-rich phenomenon, which in turn causes an imbalance in the chemical ratio of the GaAs single crystal.
[0004] Since the chemical ratio imbalance problem causes dislocation density defects in GaAs single crystals, which in turn affects the performance of the devices prepared therefrom, it is particularly important to solve the dislocation density defects of GaAs single crystals.
[0005] Therefore, it is of great significance to study and develop a new GaAs single crystal preparation method to improve the arsenic-rich phenomenon, the boron oxide layer absorbs water and decomposes B impurities, thereby reducing dislocation density defects and improving the quality of GaAs single crystals. Summary of the invention
[0006] In view of this, the technical problem to be solved by the present invention is to provide a device for preparing gallium arsenide single crystals and a method for preparing gallium arsenide single crystals. The gallium arsenide single crystals prepared by the device and method of the present invention have the advantages of high crystallization rate and low dislocation density defects.
[0007] In order to achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0008] The present invention provides a device for preparing gallium arsenide single crystal, comprising a single crystal synthesis furnace, a stepped quartz tube arranged inside the single crystal synthesis furnace, and an ultrasonic plate connected to the bottom of the single crystal synthesis furnace;
[0009] Wherein, a magnet is arranged in the single crystal synthesis furnace;
[0010] The stepped quartz tube comprises a tube body, one end of which is provided with a detachable sealing device, the sealing device is provided with a nitrogen inlet, and the other end is provided with a Y-shaped gas delivery pipe for delivering hydrogen and oxygen;
[0011] The pipe body includes two coaxially arranged lower pipe body units and an upper pipe body unit from the Y-shaped gas delivery pipe to the opening, the upper pipe body unit and the lower pipe body unit are independently circular tube-shaped, and the diameter of the lower pipe body unit is smaller than the diameter of the upper pipe body unit;
[0012] The upper tube unit is provided with a first boron nitride crucible with a conical bottom and an opening;
[0013] The lower tube unit is provided with a second boron nitride crucible with a conical bottom, and the second boron nitride crucible also includes a material cavity communicated with the conical bottom;
[0014] The material cavity is communicated with the gas outlet of the Y-shaped gas delivery pipe.
[0015] Preferably, the top diameter of the first boron nitride crucible is 100-200 mm, and the bottom opening diameter is 10-20 mm; more preferably, the top diameter of the first boron nitride crucible is 150 mm, and the bottom opening diameter is 15 mm;
[0016] Preferably, the top diameter of the second boron nitride crucible is 50-150 mm, and the diameter of the material cavity is 5-15 mm; more preferably, the top diameter of the second boron nitride crucible is 100 mm, and the diameter of the material cavity is 8 mm.
[0017] Preferably, the top and bottom of the single crystal synthesis furnace each contain two magnets, and the two top magnets form an angle of 90°-100°, and the two bottom magnets form an angle of 90°-100°; more preferably, the two top magnets form an angle of 90° or 100°, and the two bottom magnets form an angle of 90° or 100°.
[0018] The angle of the magnets is controlled by the design of the single crystal synthesis furnace. For example, if the two top magnets need to be at 90°, the top plate of the single crystal synthesis furnace must be designed to have an angle of 90°.
[0019] Preferably, the gas supply pipe on the top of the quartz cap and the Y-shaped gas supply pipe both include exhaust valves for controlling the gas delivery volume.
[0020] The present invention also provides a method for preparing a gallium arsenide single crystal, which is prepared using the above-mentioned equipment and comprises the following steps:
[0021] 1) introducing oxygen into the sealed stepped quartz tube in the single crystal synthesis furnace and heating until a dense layer of boron oxide is formed on the inner wall of the boron nitride crucible, and then introducing nitrogen to maintain the internal pressure of the stepped quartz tube at 1 atm or above;
[0022] The first boron nitride crucible in the stepped quartz tube is filled with gallium arsenide polycrystals, the material cavity is filled with gallium arsenide seed crystals, and a magnet is arranged inside the single crystal synthesis furnace;
[0023] 2) Under the action of a magnetic field, hydrogen is continuously introduced into a stepped quartz tube with an internal pressure of more than 1 atm, and the tube is heated and ultrasonically vibrated to melt the gallium arsenide polycrystal and drip onto the surface of the gallium arsenide seed crystal;
[0024] 3) The temperature gradient is controlled by a vertical gradient condensation method so that the gallium arsenide solid-liquid interface moves vertically upward from the seed crystal portion to prepare a gallium arsenide single crystal.
[0025] In the above preparation method, in step 1), oxygen is passed through the sealed stepped quartz tube and heated, so that a dense boron oxide layer is formed on the inner walls of the first and second boron nitride crucibles. The boron oxide layer can effectively prevent the gallium arsenide polycrystalline melt (obtained by melting gallium arsenide polycrystalline) at high temperature from directly contacting the inner wall of the boron nitride crucible to form twins, and at the same time avoid the introduction of B impurities to occupy Ga positions, thereby maintaining the chemical ratio balance of gallium arsenide.
[0026] Next, after the formation of the above-mentioned boron oxide layer, nitrogen is quickly introduced to cool the boron nitride crucible with the boron oxide layer on the surface to room temperature. During the cooling process, the boron oxide layer will not come into contact with moisture in the air, which reduces the water content of the boron oxide layer, thereby reducing the content of B impurities and the concentration of SiAs, etc., which helps to reduce self-compensation and improve the doping activation efficiency of Si, thereby reducing impurity deposition defects and improving the crystallization rate of gallium arsenide single crystals. Because B impurities will form a mixture with dopant Si, the intrinsic substance As and Ga compound SiAs, etc., if the B impurity is high, the concentration of the mixture with SiAs, etc. will increase, thereby agglomerating into nuclei, which is easy to produce twins and dislocation density.
[0027] In the above step 1), nitrogen is used to maintain a stable gas pressure inside the stepped quartz tube, thereby avoiding the decomposition of GaAs at high temperature. At the same time, it also replaces the method of adding single substance As in the traditional GaAs growth method, thereby reducing the arsenic enrichment phenomenon.
[0028] Then, hydrogen is continuously introduced into the stepped quartz tube with an internal pressure of more than 1 atm and heated. On the one hand, the gallium arsenide polycrystal melts and drips onto the surface of the gallium arsenide seed crystal; on the other hand, the introduced hydrogen reduces the metal impurities in the gallium arsenide polycrystal into a metal element. Due to the segregation of the metal impurities, the metal impurities in the elemental state are more likely to be biased toward the liquid phase (the liquid after the gallium arsenide polycrystal is melted, i.e., the gallium arsenide polycrystal melt). Therefore, when the vertical gradient condensation method described in step 3) is used to grow the gallium arsenide single crystal, the metal impurities will be concentrated at the tail of the crystal. The addition of hydrogen makes the internal purity of the gallium arsenide single crystal better, thereby reducing the holes formed by metal ion impurities, and reducing the stress accumulation and dislocation defects of the single crystal.
[0029] In addition, the ultrasonic vibration described in step 2) of the present invention makes the gallium arsenide particles more dispersed, and then the metal impurity element generated after hydrogen reduction is more easily gathered at the tail through the segregation effect, thereby improving the internal purity of the gallium arsenide single crystal.
[0030] In addition, the present invention adopts the above-mentioned equipment to prepare gallium arsenide single crystals, and the equipment contains magnets in the single crystal synthesis furnace.
[0031] The magnetic field generated by the magnet can control the temperature field stability of the single crystal synthesis furnace. Because the magnetic field is concentrated in the middle of the gallium arsenide polycrystalline melt, the Maranloni convection in the melt can be suppressed, and the thermal stability of the head and tail of the melt can be improved. The magnetic field can maintain the temperature stability between the crystal cone and the equal diameter part, thereby reducing the low dislocation density and crystal slip line defects, and improving the quality of gallium arsenide single crystals.
[0032] Preferably, the top and bottom of the single crystal synthesis furnace each contain two magnets, and the two top magnets form an angle of 90°-100°, and the two bottom magnets form an angle of 90°-100°; more preferably, the two top magnets form an angle of 90° or 100°, and the two bottom magnets form an angle of 90° or 100°. Because the closer the solid-liquid interface in the stepped quartz tube is to the crystal tail, the greater the temperature field of the crystal tail and crystal head of the gallium arsenide single crystal will be, and the temperature field of the crystal tail of the gallium arsenide single crystal will be affected more. Therefore, magnets are added to the top and bottom of the furnace body of the single crystal synthesis furnace at the same time, and the magnetic field is concentrated to the middle position of the gallium arsenide single crystal. The temperature field of the growth of the crystal tail of the gallium arsenide single crystal can be better maintained, and defects such as twins caused by excessive temperature differences can be reduced, thereby improving the quality of the gallium arsenide single crystal.
[0033] The present invention promotes the improvement of the quality of gallium arsenide single crystal by direct oxidation of the boron nitride crucible, passing nitrogen to maintain stable gas pressure and reduce the water content of the boron oxide layer, and increasing the temperature field stability by ultrasonic dispersion and magnetic field.
[0034] Preferably, in the method for preparing the gallium arsenide single crystal, the solid-liquid interface condensation rate of the vertical gradient condensation method in 3) is 0.8-1.2 mm / h.
[0035] Preferably, in the step 1), the mass ratio of the gallium arsenide polycrystal to the dopant silicon contained in the gallium arsenide polycrystal is (10000-15000):1.
[0036] Preferably, in the step 1), the flow rate of oxygen is 50-100 mL / min; more preferably 70-100 mL / min; further preferably 100 mL / min.
[0037] Preferably, the heating temperature in step 1) is 900°C-1000°C; more preferably 950°C.
[0038] Preferably, the flow rate of nitrogen in step 1) is 20-30 mL / min, more preferably 25-30 mL / min. In some specific embodiments of the present invention, it is preferably 30 mL / min.
[0039] Preferably, in the step 2), the heating temperature is 1240°C-1245°C.
[0040] Preferably, the heating time in step 2) is 8-16 hours; more preferably 10-16 hours.
[0041] Preferably, the flow rate of hydrogen in step 2) is 2-5 mL / min; more preferably 1 mL / min; or 2 mL / min.
[0042] Preferably, the frequency of the ultrasound in step 3) is 20-30KH. In some specific embodiments of the present invention, it is preferably 20KH or 30KH.
[0043] The present invention also provides a gallium arsenide single crystal, which is prepared by the above-mentioned preparation method;
[0044] Preferably, the crystallization rate of the gallium arsenide single crystal is 80%-90%; in some specific embodiments of the present invention, it is preferably 88%, 86%, 83% or 80%.
[0045] Preferably, the average dislocation density defect of the gallium arsenide single crystal is less than 100 / cm 2 .
[0046] The present invention also provides a material, comprising the above-mentioned gallium arsenide single crystal.
[0047] The material is used in microwave high-power devices, low-noise devices, microwave millimeter-wave monolithic integrated circuits, ultra-high-speed digital circuits and other devices.
[0048] Compared with the prior art, the equipment for preparing gallium arsenide single crystals provided by the present invention has novel functions, and the equipment can be used to prepare gallium arsenide single crystals with high crystallization rate and low dislocation density defects. The preparation method of gallium arsenide single crystals controls the temperature field stability in the furnace by the magnetic field generated by the magnet in the single crystal growth furnace, thereby ensuring the thermal stability of the gallium arsenide polycrystalline melt and significantly improving the quality of gallium arsenide single crystals. In addition, the preparation method does not require the addition of boron oxide, and directly obtains boron oxide by reacting oxygen and boron nitride crucible for sealing, and then maintains a stable air pressure inside the stepped quartz tube by nitrogen to maintain the chemical ratio balance of gallium arsenide. In addition, the preparation method also reduces holes, agglomeration and stress accumulation by reducing metal impurity ions with hydrogen and promoting the segregation of metal impurity elements with ultrasonic vibration, thereby reducing dislocation density defects and improving the crystallization rate of gallium arsenide single crystals. BRIEF DESCRIPTION OF THE DRAWINGS
[0049] Figure 1 Schematic diagram of a stepped quartz tube, wherein 1-1 is a hydrogen gas delivery pipe, 1-2 is an oxygen gas delivery pipe, 1-3 is a quartz tube exhaust valve, 1-4 is a quartz bottom gas delivery pipe, and 1-5 is a trapezoidal quartz tube body;
[0050] Figure 2 Schematic diagram of a stepped quartz tube containing a boron nitride crucible, wherein 2-1 is a material chamber, 2-2 is a small-diameter boron nitride crucible, and 2-3 is a large-diameter boron nitride crucible;
[0051] Figure 3 Schematic diagram of the device after loading gallium arsenide polycrystal and seed crystal, wherein 3-1 is gallium arsenide seed crystal, and 3-2 is gallium arsenide polycrystal;
[0052] Figure 4 Schematic diagram of the stepped quartz tube after loading and sealing, wherein 4-1 is the welding point between the quartz tube and the quartz cap, 4-2 is the quartz cap, 4-3 is the nitrogen gas delivery pipe, and 4-4 is the quartz cap exhaust valve;
[0053] Figure 5 The device diagram for preparing gallium arsenide single crystal of the present invention, wherein 5-1 is a quartz support tube, 5-2 is a single crystal growth furnace, 5-3 is a heater, 5-4 is an ultrasonic plate, 5-5 is a magnet at the bottom of the crystal growth furnace, and 5-6 is a magnet at the top of the crystal growth furnace;
[0054] Figure 6 Schematic diagram of equipment for preparing gallium arsenide single crystal in Comparative Example 1;
[0055] Figure 7 Schematic diagram of the equipment for preparing gallium arsenide single crystal in comparative example 2. DETAILED DESCRIPTION
[0056] In order to further illustrate the present invention, the equipment for preparing gallium arsenide single crystal and the method for preparing gallium arsenide single crystal provided by the present invention are described in detail below in conjunction with embodiments.
[0057] use Figure 1-5 The equipment is used to prepare gallium arsenide single crystals, specifically comprising the following steps:
[0058] 1) placing gallium arsenide polycrystals into the first boron nitride crucible (as shown in 2-3) having a conical bottom and an opening, placing gallium arsenide seed crystals into the material cavity (as shown in 2-1) of the second boron nitride crucible (as shown in 2-2) having a conical bottom and including a material cavity connected to the conical bottom, and then placing a quartz cap (as shown in 4-2) on the top of the stepped quartz tube ( Figure 1 The upper and lower parts (including the top) are sealed and connected and placed as a whole in a single crystal synthesis furnace (as shown in 5-2);
[0059] 2) heating the stepped quartz tube and introducing oxygen into it (via Figure 1 1-1) until a dense layer of boron oxide forms on the inner wall of the boron nitride crucible, and then nitrogen is introduced (through Figure 1 The oxygen gas delivery pipe shown in 1-2 is introduced to keep the internal pressure of the stepped quartz tube above 1atm;
[0060] 3) Continuously introduce hydrogen into a stepped quartz tube with an internal pressure of more than 1 atm and heat it (heated by the heater shown in 5-3 in the single crystal synthesis furnace) to melt the gallium arsenide polycrystal and drip it onto the surface of the gallium arsenide seed crystal;
[0061] 4) Starting the ultrasonic plate (as shown in 5-4) to ultrasonically process the stepped quartz tube to prepare a gallium arsenide single crystal.
[0062] Example 1
[0063] The first step: prepare clean and dried trapezoidal quartz tube and boron nitride crucible, put the boron nitride crucible into the quartz tube, wherein the small-diameter boron nitride crucible (i.e., the second boron nitride crucible with a conical bottom and a material cavity connected to the conical bottom) is placed at the lower part of the quartz tube (lower tube unit), and the large-diameter boron nitride crucible (i.e., the first boron nitride crucible with a conical bottom and an opening) is placed at the upper part of the quartz tube (upper tube unit), as shown in FIG. Figure 1 and Figure 2 ;
[0064] Step 2: Place the GaAs seed crystal in the seed crystal cavity of the small diameter boron nitride crucible, and then put 12 kg of GaAs polycrystalline material into the large diameter boron nitride crucible. Figure 3 As shown;
[0065] Step 3: Use hydrogen-oxygen flame to vertically weld the quartz cap and the stepped quartz tube together to make the stepped quartz tube and the quartz cap sealed. Figure 4 As shown;
[0066] Step 4: Put the welded stepped quartz tube into the single crystal growth furnace (also called crystal growth furnace or single crystal synthesis furnace), use a quartz support tube to vertically support the quartz tube at the bottom of the furnace, cover the single crystal growth furnace, make the quartz tube completely in the single crystal growth furnace, and the gas pipes at the bottom and top of the quartz tube pass through the single crystal growth furnace;
[0067] Step 5: Place two magnets at the bottom and top of the single crystal growth furnace, with the two magnets at the bottom forming a 90° angle and the two magnets at the top forming a 90° angle. Figure 5 As shown;
[0068] Step 6: Continue to flush oxygen from the oxygen gas pipe at the bottom of the quartz tube, control the oxygen flow rate at 100mL / min, heat to 950℃, and maintain for 30 minutes to form a dense layer of boron oxide on the inner wall of the boron nitride crucible;
[0069] Step 7: Turn off the oxygen, and at the same time, introduce nitrogen from the nitrogen gas pipe on the top of the quartz tube, then open the exhaust valve of the quartz tube to remove the residual oxygen, and continue to introduce nitrogen. The nitrogen flow rate is controlled at 30mL / min, and the air pressure in the quartz tube is kept above 1atm;
[0070] Step 8: Turn off the nitrogen, introduce hydrogen from the hydrogen gas pipe at the bottom of the quartz tube, open the exhaust valve of the quartz cap to exhaust the nitrogen, then close the exhaust valve of the quartz cap and continue to add hydrogen. The hydrogen flow rate is controlled at 2mL / min, and the melting process is kept in the hydrogen state;
[0071] Step 9: Heat to 1240℃-1245℃ to melt the polycrystalline material in the quartz tube and drip into the small diameter crucible at the bottom; after the gallium arsenide polycrystalline material is melted, continue heating for 16 hours, start the ultrasonic plate at the bottom of the single crystal growth furnace, and control the frequency at 30KH.
[0072] Step 10: After the melting of the gallium arsenide polycrystalline material is completed, the ultrasonic vibration is stopped, and the temperature gradient is controlled so that the solid-liquid interface condensation rate is 1mm / h. Starting from the seed crystal part, it is controlled at 1238℃, so that the gallium arsenide solid-liquid interface moves vertically upward from the seed crystal part, and finally grows a crystal with low stress concentration and low dislocation density defects.
[0073] The top diameter of the first boron nitride crucible is 150 mm, and the bottom opening diameter is 15 mm; the top diameter of the second boron nitride crucible is 100 mm, and the diameter of the material cavity is 8 mm.
[0074] Example 2
[0075] This embodiment provides a gallium arsenide single crystal. The only difference between the gallium arsenide single crystal growth method and the embodiment 1 is that in the seventh step, the hydrogen flow rate is controlled at 1 mL / min.
[0076] Example 3
[0077] This embodiment provides a gallium arsenide single crystal. The only difference between the gallium arsenide single crystal growth method and embodiment 1 is that in the ninth step, the gallium arsenide polycrystalline material is continuously heated for 8 hours after melting, and the ultrasonic plate at the bottom of the single crystal growth furnace is started, and the frequency is controlled at 20KH.
[0078] Example 4
[0079] This embodiment provides a gallium arsenide single crystal. The difference between the gallium arsenide single crystal growth method and the embodiment 1 is that in the fourth step, two magnets are placed at the bottom and the top of the single crystal growth furnace, and the two magnets form an angle of 100 degrees.
[0080] Comparative Example 1
[0081] The difference between Comparative Example 1 and Example 1 is that in step 5, no magnets are placed at the bottom and top of the single crystal growth furnace. Figure 6 As shown, and Figure 5 Compared with the device shown in the figure, the difference is that the single crystal synthesis furnace does not contain magnets.
[0082] Comparative Example 2
[0083] Comparative Example 2 is different from Example 1 in that in step 9, no ultrasonic plate is placed at the bottom of the single crystal growth furnace. Figure 7 As shown, and Figure 5 Compared with the device shown in the figure, the difference is that the bottom outside the single crystal synthesis furnace is not connected to the ultrasonic plate.
[0084] Comparative Example 3
[0085] Comparative Example 3 is different from Example 1 in that in step 8, no hydrogen is added after the quartz cap exhaust valve is closed.
[0086] Comparative Example 4
[0087] Comparative Example 4 differs from Example 1 in that in the fifth step, magnets are provided at the bottom and top of the single crystal growth furnace, but the two magnets at the bottom form an angle of 60°, and the two magnets at the top form an angle of 180°. Specifically, the angle is controlled by designing the single crystal synthesis furnace. If the furnace top is made horizontal, the top magnet is 180°, and if the bottom of the single crystal furnace is made at an angle of 60°, the magnet can be controlled to be 60°. Table 1 Dislocation density defects and crystallization rate of gallium arsenide single crystals prepared by Examples 1 to 4 and Comparative Examples 1 to 3
[0088]
[0089] By comparing Example 1 and Example 2, the results show that reducing the hydrogen flow rate increases the dislocation density defect (EPD) and decreases the crystallization rate; comparing Example 1 and Comparative Example 3, when no hydrogen is introduced, the EPD increases by nearly 10 times and the crystallization rate also decreases by nearly 10%;
[0090] Comparing Example 1 with Example 3, by shortening the polycrystalline melting time and reducing the ultrasonic frequency, the EPD increased to nearly 2 times of the original value, and the crystallization rate also decreased by nearly 8%;
[0091] Comparing Example 1 and Comparative Example 2, the polycrystalline material was not subjected to ultrasonic action during the melting process, and the EDP increased by nearly 10 times, and the crystallization rate decreased by 9%;
[0092] Comparing Example 1 and Example 4, when the angle between the two magnets at the bottom and top of the single crystal growth furnace increases, the EPD will increase slightly, and the crystallization rate will decrease by nearly 2%;
[0093] By comparing Example 1 with Comparative Example 1, in which no magnets are placed at the bottom and top of the single crystal growth furnace, the EPD of the single crystal head increases significantly, by nearly 30 times, and the overall crystallization rate also decreases by nearly 12%.
[0094] Comparing Example 1 and Comparative Example 4, when the direction of the magnetic field changes, that is, the angle between the bottom and top magnets inside the single crystal growth furnace changes, when the angle is small (smaller than the range described in the present invention), the attraction is strong and the magnetic field is concentrated; when the angle increases (larger than the range described in the present invention), the attraction is dispersed; both are not conducive to the temperature field stability in the single crystal growth furnace and the thermal stability of the gallium arsenide polycrystalline melt, resulting in a decrease in the quality of the gallium arsenide single crystal.
[0095] Through the above-mentioned embodiments and comparative examples, the results show that the gallium arsenide single crystal prepared by the present invention has a smaller dislocation density and a higher crystallization rate.
[0096] The above embodiments are only used to help understand the method and core idea of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made to the present invention without departing from the principles of the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.
Claims
1. A device for preparing gallium arsenide single crystal, characterized in that: It includes a single crystal synthesis furnace, a stepped quartz tube arranged inside the furnace, and an ultrasonic plate connected to the bottom of the single crystal synthesis furnace; Wherein, a magnet is arranged in the single crystal synthesis furnace; The stepped quartz tube comprises a tube body, one end of which is provided with a detachable sealing device, the sealing device is provided with a nitrogen inlet, and the other end is provided with a Y-shaped gas delivery pipe for delivering hydrogen and oxygen; The pipe body includes two coaxially arranged lower pipe body units and an upper pipe body unit from the Y-shaped gas delivery pipe to the opening, the upper pipe body unit and the lower pipe body unit are independently circular tube-shaped, and the diameter of the lower pipe body unit is smaller than the diameter of the upper pipe body unit; The upper tube unit is provided with a first boron nitride crucible with a conical bottom and an opening; The lower tube unit is provided with a second boron nitride crucible with a conical bottom, and the second boron nitride crucible also includes a material cavity communicated with the conical bottom; The material cavity is communicated with the gas outlet of the Y-shaped gas delivery pipe.
2. The device according to claim 1, characterized in that The top and bottom of the single crystal synthesis furnace each contain two magnets, and the two magnets on the top form an angle of 90°-100°, and the two magnets on the bottom form an angle of 90°-100°.
3. A method for preparing a gallium arsenide single crystal, characterized in that: The preparation is carried out using the device described in claim 1 or 2, comprising the following steps: 1) introducing oxygen into the sealed stepped quartz tube in the single crystal synthesis furnace and heating until a dense layer of boron oxide is formed on the inner wall of the boron nitride crucible, and then introducing nitrogen to maintain the internal pressure of the stepped quartz tube at 1 atm or above; The first boron nitride crucible in the stepped quartz tube is filled with gallium arsenide polycrystals, the material cavity is filled with gallium arsenide seed crystals, and a magnet is arranged inside the single crystal synthesis furnace; 2) Under the action of a magnetic field, hydrogen is continuously introduced into a stepped quartz tube with an internal pressure of more than 1 atm, and the tube is heated and ultrasonically vibrated to melt the gallium arsenide polycrystal and drip onto the surface of the gallium arsenide seed crystal; 3) The temperature gradient is controlled by a vertical gradient condensation method so that the gallium arsenide solid-liquid interface moves vertically upward from the seed crystal portion to prepare a gallium arsenide single crystal.
4. The preparation method according to claim 3, characterized in that: The solid-liquid interface condensation rate of the vertical gradient condensation method in 3) is 0.8-1.2 mm / h.
5. The preparation method according to claim 3, characterized in that: In the step 1), the mass ratio of the gallium arsenide polycrystal to the dopant silicon element contained in the gallium arsenide polycrystal is (10000-15000):
1.
6. The preparation method according to claim 3, characterized in that: The flow rate of oxygen in step 1) is 50-100 mL / min; The heating temperature in step 1) is 900° C.-1000° C.; The flow rate of nitrogen in step 1) is 20-30 mL / min.
7. The preparation method according to claim 3, characterized in that: The heating temperature in step 2) is 1240°C-1245°C; The heating time in step 2) is 8-16 hours; The flow rate of hydrogen in step 2) is 2-5 mL / min.
8. The preparation method according to claim 3, characterized in that: The frequency of the ultrasound in step 3) is 20-30KH.
9. A gallium arsenide single crystal, characterized in that: Prepared by the preparation method according to any one of claims 3 to 8; The crystallization rate of the gallium arsenide single crystal is 80%-90%; The average dislocation density defect of the gallium arsenide single crystal is less than 100 / cm 2 .
10. A material, characterized in that Comprising the gallium arsenide single crystal as described in claim 9.