Antibacterial fabric containing alginate fibers and preparation method thereof

By adding seaweed fibers and toughening treatment agents to the regenerated cellulose fiber fabric to form antibacterial yarn, the problem of bacteria and wear after sweat erosion in high temperature climates is solved, and the durability and antibacterial properties of the fabric are improved.

CN118979332AActive Publication Date: 2024-11-19GUANGDONG QIYUE FUTURE TECH CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411059302.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-03
Publication Date
2024-11-19
Estimated Expiration
2044-08-03

AI Technical Summary

Technical Problem

Regenerated cellulose fiber fabrics are prone to bacterial growth, wear and pilling after long-term use, reducing the durability and safety of fitted clothing, especially after sweat erosion in high temperature climates.

Method used

85-92% regenerated cellulose fibers are combined with 8-15% seaweed fibers to form antibacterial yarns and treated with toughening treatment agents, including methoxy polyethylene glycol acrylate and (3-methacryloyloxy Compositions such as 2-hydroxypropoxy)propylbis(trimethylsiloxy)methyl, methacryloylethylsulfobetaine, etc., form macromolecular polymers and enhance tensile strength and adhesion , form an antibacterial toughening membrane to reduce wear and fracture.

Benefits of technology

It improves the durability and safety of antibacterial fabrics, enhances antibacterial and toughness, reduces bacteria and wear after sweat erosion, and extends the service life of the fabric.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004977342970000041
    Figure BDA0004977342970000041
  • Figure BDA0004977342970000051
    Figure BDA0004977342970000051
  • Figure BDA0004977342970000081
    Figure BDA0004977342970000081
Patent Text Reader

Abstract

The invention relates to the technical field of textile fabrics, in particular to an antibacterial fabric containing alginate fibers and a preparation method of the antibacterial fabric. The fabric is obtained by knitting antibacterial yarns, the antibacterial yarns are composed of 85-92% by mass of regenerated cellulose fibers and 8-15% by mass of alginate fibers, and the number of the antibacterial yarns is 30-40. The antibacterial yarn obtained by compounding 85-92% of regenerated cellulose fibers and 8-15% of alginate fibers has the comprehensive performance of the regenerated cellulose fibers and the alginate fibers, the number of the antibacterial yarn is 30-40, and under the component composition and count range of the antibacterial yarn, the obtained antibacterial fabric has better wear resistance, antibacterial property and softness, the phenomena of pilling, bacterium breeding and the like are reduced, and the antibacterial fabric is worthy of popularization and application. The good deodorization effect and the good moisture removal effect are achieved, and the safety and durability of the clothes in the using process are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of textile fabrics, and more specifically, to an antibacterial fabric containing seaweed fibers and a preparation method thereof. Background Art

[0002] Regenerated cellulose fiber is a textile fiber made from natural cellulose by changing its physical structure. Regenerated cellulose fiber has excellent properties such as environmental protection, breathability, moisture absorption, skin-friendly and comfortable, and dyeing performance, so it is widely used in fabric manufacturing. The manufactured fabrics are widely used in pajamas, underwear, panties and other intimate clothing.

[0003] However, with global warming, especially in summer, the average temperature in various places has increased significantly. Therefore, it is easy to sweat when outdoors. After a large amount of sweat is discharged, it is easy to soak the underwear, thereby reducing the comfort of wearing clothes.

[0004] At the same time, if clothes with sweat are not washed in time, they are easy to breed bacteria, which will cause the clothes to change color, stink, wear and tear, etc., reducing the safety and durability of underwear. Further research is needed for this. Summary of the invention

[0005] In order to solve the above technical problems, the present application provides an antibacterial fabric containing seaweed fiber and a preparation method thereof.

[0006] In a first aspect, the present application provides an antibacterial fabric containing seaweed fiber, which is obtained by knitting antibacterial yarn, wherein the antibacterial yarn component is composed of 85-92% by mass of regenerated cellulose fiber and 8-15% by mass of seaweed fiber, and the antibacterial yarn is 30-40 counts.

[0007] In the above scheme, seaweed fiber has good moisture absorption performance, and exerts its moisture absorption performance through contact with the skin, actively releasing seaweed components, thereby improving the antibacterial and deodorizing effects of the antibacterial fabric. Therefore, the antibacterial yarn formed by regenerated cellulose fiber and seaweed fiber has good antibacterial properties. The antibacterial fabric obtained by knitting has good air permeability, antibacterial and moisture discharge properties. When wearing clothes, it can achieve rapid perspiration and reduce the growth of bacteria on clothes. The antibacterial property of this application is as high as 99%.

[0008] Furthermore, the antibacterial yarn obtained by compounding 85-92% of regenerated cellulose fiber and 8-15% of seaweed fiber has the comprehensive performance of the two, so the obtained fabric has the characteristics of better strength, antibacterial property, softness and comfort, and the antibacterial yarn is selected to be 30-40 counts. Under the component composition and count range of the antibacterial yarn, the obtained antibacterial fabric has better wear resistance, antibacterial property and softness, reduces the occurrence of pilling, bacterial growth and the like, and has better deodorization and moisture removal effects, thereby improving the safety and durability of the clothes during use.

[0009] Preferably, the fabric weight is 100-150g / m 3 .

[0010] When the weight is 100-150g / m 3 At the same time, the fabric has better air permeability, moisture discharge, softness, comfort and wear resistance, which further reduces the possibility of bacteria breeding on the antibacterial fabric and improves the safety, durability and comfort of wearing clothing.

[0011] Preferably, the antibacterial yarn is treated with a toughening agent, and the toughening agent is composed of the following raw materials in parts by weight: 20-30 parts water 1-5 parts of environmentally friendly organic solvent Antibacterial viscosity enhancer 0.8-1.7 parts Emulsifier 0.5-1 part Ammonium persulfate 0.1-0.3 parts Methoxy polyethylene glycol acrylate 0.01-0.08 parts Methacryloylethyl sulfobetaine 0.5-1.8 parts (3-methacryloyloxy-2-hydroxypropoxy)propyl bis(trimethylsilyloxy)methyl 0.1-0.5 parts.

[0012] Although seaweed fiber can improve antibacterial and hygroscopic properties, its strength is relatively weak. Therefore, the antibacterial yarn produced is prone to drawing and fiber breakage during the textile process, causing the surface of the fabric to become fuzzy. In addition, after long-term use, the surface of underwear made of antibacterial fabrics is still prone to bacteria breeding, wear and pilling, thereby reducing the durability and safety of the antibacterial fabric.

[0013] To this end, the present application further uses a toughening agent for treatment to improve the tightness of the seaweed fiber and the regenerated cellulose in the antibacterial yarn, reduce the possibility of wear and pilling of the antibacterial fabric after long-term use, and improve the durability of the antibacterial fabric. At the same time, it has a better antibacterial effect and reduces the possibility of bacteria breeding, wear and pilling after the fabric is eroded by sweat.

[0014] Specifically, methoxy polyethylene glycol acrylate can enhance tensile strength and ductility, and improve the toughness of the antibacterial treatment agent after film formation; while methacryloylethyl sulfobetaine has wettability, dispersibility, and antibacterial properties, and at the same time contains methacrylic acid groups, which are copolymerized with methoxy polyethylene glycol acrylate and (3-methacryloyloxy-2-hydroxypropoxy)propylbis(trimethylsilyloxy)methyl to form a macromolecular polymer with better adhesion, film-forming properties and toughness after film formation.

[0015] The (3-methacryloyloxy-2-hydroxypropoxy)propyl bis(trimethylsilyloxy)methyl molecule contains hydroxyl, silyl and acrylate groups, which further react with methacryloylethyl sulfobetaine and methoxypolyethylene glycol acrylate to form a macromolecular polymer with good adhesion and film-forming properties.

[0016] Therefore, through the copolymerization reaction of methoxy polyethylene glycol acrylate, (3-methacryloyloxy-2-hydroxypropoxy)propyl bis(trimethylsiloxy)methyl, and methoxy polyethylene glycol acrylate, a macromolecular polymer is formed, and then interacts with the antibacterial thickener, so that the prepared toughening treatment agent has better antibacterial properties, adhesion, film-forming properties and film-forming toughness. Therefore, after the antibacterial yarn is treated, it can penetrate into the gap between the seaweed fiber and the cellulose fiber. After curing, the seaweed fiber and the cellulose fiber are stably adhered and an antibacterial toughening film is formed on the surface of the antibacterial yarn. Therefore, the possibility of wear, pilling, breakage, etc. of the prepared antibacterial fabric can be reduced, and the durability of the antibacterial fabric can be improved.

[0017] In addition, since the antibacterial thickener and methacryloylethyl sulfobetaine both have good antibacterial properties, the two work together to make the toughening agent have good antibacterial effect. After the antibacterial yarn is treated, the antibacterial yarn has good antibacterial and toughness, reducing the possibility of wear, breakage, pilling, etc., and improving the safety and durability of the antibacterial fabric.

[0018] Furthermore, the macromolecular polymer formed by copolymerization of methoxy polyethylene glycol acrylate, (3-methacryloyloxy-2-hydroxypropoxy)propyl bis(trimethylsilyloxy)methyl and methoxy polyethylene glycol acrylate has sweat resistance, which reduces the antibacterial fabric from being eroded by sweat. At the same time, it is combined with antibacterial thickeners, methacryloylethyl sulfobetaine, etc. to further enhance the antibacterial property of the antibacterial yarn, so that the obtained antibacterial fabric has better sweat resistance, antibacterial and wear resistance, and reduces the possibility of bacteria breeding, easy wear and pilling after being eroded by sweat.

[0019] The treatment process of the toughening agent for antibacterial yarn is as follows: Weigh ammonium persulfate, (3-methacryloyloxy-2-hydroxypropoxy)propyl bis(trimethylsiloxy)methyl, methoxypolyethylene glycol acrylate, methacryloylethyl sulfobetaine, an emulsifier and water, mix them evenly, heat to 62-70°C, react for 1-2 hours, then add an antibacterial thickener and an environmentally friendly organic solvent, stir for 1-2 hours to obtain a toughening treatment agent; soak the weighed antibacterial yarn in the toughening treatment agent for 10-30 minutes, and dry it to obtain the antibacterial yarn after reinforcement treatment.

[0020] In the above process, (3-methacryloyloxy-2-hydroxypropoxy)propyl bis(trimethylsiloxy)methyl, methoxypolyethylene glycol acrylate and methacryloylethyl sulfobetaine are compounded, and with the assistance of water, emulsifier and ammonium persulfate, the active groups are further reacted and copolymerized by heating, and then the antibacterial thickener is added to further thicken the toughening system, so that after the prepared treatment agent is used to treat the antibacterial yarn, the toughness of the antibacterial yarn is further improved, so that the obtained antibacterial fabric has better antibacterial properties, wear resistance, soft feel and the like.

[0021] Preferably, the antibacterial viscosity enhancing agent is one or more of mussel mucin, polyglutamic acid, and chitosan derivatives.

[0022] Mussel mucin, polyglutamic acid and chitosan derivatives all have certain antibacterial effects, and they are filled in the toughening agent to play a viscosity-increasing role, further improving the toughness and antibacterial properties of the antibacterial yarn treated with the toughening agent.

[0023] Preferably, the antibacterial viscosity enhancing agent consists of mussel mucin, polyglutamic acid, and chitosan derivatives.

[0024] When mussel mucin, polyglutamic acid and chitosan derivatives are used in combination, they have better antibacterial effect and thickening effect. After the toughening agent is used to treat the antibacterial yarn, the antibacterial yarn has better antibacterial property and toughness, reducing the possibility of antibacterial yarn breakage, pilling and wear during the production process or in the use process, and at the same time making the antibacterial fabric have better antibacterial property.

[0025] Preferably, the weight ratio of the mussel mucin, polyglutamic acid and chitosan derivative is (3-8):3:(2-7).

[0026] Preferably, the chitosan derivative is sulfonated chitosan and / or methacrylylated chitosan.

[0027] The weight ratio of the sulfonated chitosan to the methacrylylated chitosan is 1:(1-3) Preferably, the emulsifier is one or more of cocamidopropyl betaine, OP-10, OP-20, and sodium lauryl sulfate.

[0028] Preferably, the environmentally friendly organic solvent is anhydrous ethanol and / or dipropylene glycol dimethyl ether.

[0029] In a second aspect, the present application provides a method for preparing an antibacterial fabric containing seaweed fiber, comprising the following steps: twisting the seaweed fiber and regenerated cellulose fiber to obtain antibacterial yarn; and knitting the antibacterial yarn to obtain the antibacterial fabric.

[0030] In summary, this application has the following beneficial effects: 1. The antibacterial yarn obtained by compounding 85-92% regenerated cellulose fiber and 8-15% seaweed fiber has the comprehensive performance of both. Therefore, the obtained fabric has the characteristics of better strength, antibacterial property, softness and comfort, and the antibacterial yarn is selected to be 30-40 counts. Under the composition and count range of the antibacterial yarn, the obtained antibacterial fabric has better wear resistance, antibacterial property and softness, reduces the occurrence of pilling and bacterial growth, and has better deodorization and moisture removal effects, thereby improving the safety and durability of the clothes during use.

[0031] 2. Through the copolymerization reaction of methoxy polyethylene glycol acrylate, (3-methacryloyloxy-2-hydroxypropoxy)propyl bis(trimethylsiloxy)methyl and methoxy polyethylene glycol acrylate, a macromolecular polymer is formed, and then interacts with the antibacterial thickener, so that the prepared toughening treatment agent has better antibacterial properties, adhesion, film-forming properties and film-forming toughness. Therefore, after the antibacterial yarn is treated, it can penetrate into the gap between the seaweed fiber and the cellulose fiber. After curing, the seaweed fiber and the cellulose fiber are stably adhered and an antibacterial toughening film is formed on the surface of the antibacterial yarn. Therefore, the possibility of wear, pilling, breakage, etc. of the prepared antibacterial fabric can be reduced, and the durability of the antibacterial fabric can be improved. DETAILED DESCRIPTION

[0032] The present application is further described in detail below in conjunction with embodiments.

[0033] Introduction table of some raw materials; Table 1 Introduction of some raw materials Example

[0034] Example 1 The preparation of an antibacterial fabric containing seaweed fiber comprises the following steps: The seaweed fiber and the regenerated cellulose fiber are twisted by a twisting device to form an antibacterial yarn with a twist of 700 twists / meter. The antibacterial yarn is knitted by a knitting device in a plain needle knitting method to obtain an antibacterial fabric.

[0035] The antibacterial yarn is composed of 85% by mass of regenerated cellulose fiber and 15% by mass of seaweed fiber. The antibacterial yarn is 30 counts. The weight of the antibacterial fabric is 150g / m 3 .

[0036] Example 2 The difference between Example 2 and Example 1 is that the antibacterial yarn component is composed of 87.6% by mass of regenerated cellulose fiber and 12.4% by mass of seaweed fiber, the antibacterial yarn is 35 counts; the weight of the fabric is 128g / m 3 .

[0037] Example 3 The difference between Example 3 and Example 1 is that the antibacterial yarn component is composed of 87.6% by mass of regenerated cellulose fiber and 12.4% by mass of seaweed fiber, the antibacterial yarn is 40 counts; the weight of the fabric is 100 g / m 3 .

[0038] Example 4 The difference between Example 4 and Example 1 is that the antibacterial yarn is an antibacterial yarn treated with a toughening agent, and the specific process is as follows: Weigh 0.1 kg of ammonium persulfate, 0.1 kg of (3-methacryloyloxy-2-hydroxypropoxy)propyl bis(trimethylsilyloxy)methyl, 0.01 kg of methoxy polyethylene glycol acrylate, 0.5 kg of methacryloylethyl sulfobetaine, 0.5 kg of emulsifier, and 20 kg of water into a reactor, stir at a speed of 100 r / min for 10 min to fully mix, heat to 65 ° C, react for 90 min, then add 1.8 kg of antibacterial thickener and 5 kg of environmentally friendly organic solvent, adjust the pH value to 7, and continue stirring for 2 hours to obtain a toughening treatment agent; The weighed antibacterial yarn was immersed in a tank containing a toughening agent, wherein the temperature of the toughening agent was 40°C, and the soaking time was 15 minutes. After being taken out, it was placed in a liquid scraping device, and the toughening agent suspended on the surface of the antibacterial yarn was placed in a drying device at 80°C for drying for 5 minutes to obtain the antibacterial yarn after reinforcement treatment.

[0039] The average weight of the toughened antibacterial yarn is 5% higher than that of the untoughened antibacterial yarn, and the average gram weight of the antibacterial fabric made of the toughened antibacterial yarn is also 5% higher than that of the untoughened antibacterial yarn.

[0040] Among them, the emulsifier is cocamidopropyl betaine; the antibacterial thickener is mussel mucin; and the environmentally friendly organic solvent is anhydrous ethanol.

[0041] Example 5 The difference between Example 5 and Example 4 is that the amount of raw materials used in the treatment agent is different, specifically as follows: 0.2 kg of ammonium persulfate, 0.3 kg of (3-methacryloyloxy-2-hydroxypropoxy)propyl bis(trimethylsiloxy)methyl, 0.05 kg of methoxypolyethylene glycol acrylate, 1 kg of methacryloylethyl sulfobetaine, 0.8 kg of emulsifier, 25 kg of water, 1.3 kg of antibacterial thickener and 3 kg of environmentally friendly organic solvent.

[0042] Example 6 The difference between Example 6 and Example 4 is that the amount of raw materials used in the toughening treatment agent is different, specifically as follows: 0.3 kg of ammonium persulfate, 0.5 kg of (3-methacryloyloxy-2-hydroxypropoxy)propyl bis(trimethylsiloxy)methyl, 0.05 kg of methoxypolyethylene glycol acrylate, 1 kg of methacryloylethyl sulfobetaine, 0.8 kg of emulsifier, 25 kg of water, 0.8 kg of antibacterial thickener and 1 kg of environmentally friendly organic solvent.

[0043] Example 7 The difference between Example 7 and Example 5 is that the antibacterial viscosity enhancing agent is polyglutamic acid.

[0044] Example 8 The difference between Example 8 and Example 5 is that the antibacterial viscosity enhancing agent is a chitosan derivative (sulfonated chitosan).

[0045] Example 9 The difference between Example 9 and Example 5 is that the antibacterial viscosity enhancer consists of 1 kg of mussel mucin and 0.3 kg of polyglutamic acid.

[0046] Example 10 The difference between Example 10 and Example 5 is that the antibacterial viscosity enhancer is composed of 0.8 kg of chitosan derivative (sulfonated chitosan) and 0.5 kg of polyglutamic acid.

[0047] Embodiment 11 The difference between Example 11 and Example 5 is that the antibacterial viscosity enhancer consists of 0.3 kg of mussel mucin, 0.3 kg of polyglutamic acid, and 0.7 kg of chitosan derivative (sulfonated chitosan).

[0048] Example 12 The difference between Example 12 and Example 5 is that the antibacterial viscosity enhancer consists of 0.5 kg of mussel mucin, 0.3 kg of polyglutamic acid, and 0.5 kg of chitosan derivative (sulfonated chitosan).

[0049] Embodiment 13 The difference between Example 13 and Example 5 is that the antibacterial viscosity enhancer consists of 0.8 kg of mussel mucin, 0.3 kg of polyglutamic acid, and 0.2 kg of chitosan derivative (sulfonated chitosan).

[0050] Embodiment 14 The difference between Example 14 and Example 12 is that the chitosan derivative is methacryloyl chitosan.

[0051] Embodiment 15 The difference between Example 15 and Example 12 is that the chitosan derivative consists of 0.4 kg of sulfonated chitosan and 0.1 kg of methacryloyl chitosan.

[0052] Example 16 The difference between Example 16 and Example 4 is that the antibacterial viscosity enhancer is replaced by water in equal amounts.

[0053] Embodiment 17 The difference between Example 17 and Example 4 is that an equal amount of methoxy polyethylene glycol acrylate is replaced by methacryloylethyl sulfobetaine.

[0054] Embodiment 18 The difference between Example 18 and Example 4 is that methacryloylethyl sulfobetaine is replaced by (3-methacryloyloxy-2-hydroxypropoxy)propylbis(trimethylsilyloxy)methyl in an equal amount.

[0055] Embodiment 19 The difference between Example 19 and Example 4 is that (3-methacryloyloxy-2-hydroxypropoxy)propylbis(trimethylsilyloxy)methyl is replaced by methacryloylethylsulfobetaine in equal amounts.

[0056] Embodiment 20 The difference between Example 20 and Example 4 is that (3-methacryloyloxy-2-hydroxypropoxy)propylbis(trimethylsilyloxy)methyl is replaced by triisopropylsilylmethacrylate in an equal amount.

[0057] Comparative Example Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that the antibacterial yarn component consists of 70% by mass of regenerated cellulose fiber and 30% by mass of seaweed fiber.

[0058] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that the antibacterial yarn component consists of 95% by mass of regenerated cellulose fiber and 5% by mass of seaweed fiber.

[0059] Performance testing Detection method / test method Antibacterial property: The detection was carried out with reference to GB / T 20944.2-2007. The control group was a fabric with 100% by mass of regenerated cellulose fiber. After adding seaweed fiber, the increase in antibacterial rate of the antibacterial fabrics of Examples 1-20 and Comparative Examples 1-2 was calculated compared with the control group.

[0060] The wear-resistant microfiber fabrics obtained in Examples 1-20 and Comparative Examples 1-3 were cut into 4 groups of samples respectively. The samples were soaked in artificial sweat with a pH of 6 for 2 hours, and then the water was wrung out. The humidity of the samples was measured to be 37%. The samples were naturally dried for 36 hours at a natural drying temperature of 30°C, a humidity of 62%, and a wind speed of 0.5 m / s to obtain test samples.

[0061] (1) Integrity: Observe whether there are spots, obvious discoloration, etc. on the surface of the test sample. If the above phenomena occur, it is recorded as unqualified; if not, it is recorded as qualified.

[0062] (2) Wear degree: Refer to ISO12947-1-1998 and use Martindale wear and abrasion tester to test the test samples. The pressure is 10 kPa and the speed is 50 r / min. The friction times are 1100 times, 2000 times, 3000 times and 4500 times respectively. Then the friction degree is evaluated. The friction degree is slight wear, moderate wear and severe wear. When damage occurs, it is recorded as wear and tear, and no friction test is performed. The relevant friction degree is recorded.

[0063] The above tests are shown in Table 2. Table 2 Experimental data of Examples 1-20 and Comparative Examples 1-3 Combining Example 1 and Comparative Examples 1-2 and Table 2, it can be seen that the increase in the antibacterial rate of Comparative Example 1 is higher than that of Example 1, but Comparative Example 1 shows abrasion when the number of frictions is 3000 times, while Example 1 shows abrasion after 4500 times; the increase in the antibacterial rate of Comparative Example 2 is lower than that of Example 1, and the degree of wear of Comparative Example 2 during the friction process of 1100-4500 times is the same as that of the example, indicating that the antibacterial fabric prepared by using the seaweed fiber content range of the present application has better antibacterial and tear resistance.

[0064] Combining Example 1 and Examples 4-6 and Table 2, it can be seen that the increase in the antibacterial rate of Examples 4-6 is slightly lower than the increase in the antibacterial rate of Example 1, but the degree of wear of Examples 4-6 during the friction process of 1100-4500 times is better than that of Example 1, indicating that the toughening treatment agent prepared in the present application is used to treat the antibacterial yarn, which can reduce the occurrence of wear and other phenomena.

[0065] Combining Example 5 and Examples 10-12 and Table 2, it can be seen that the increase in the antibacterial rate of Examples 10-12 is higher than that of Example 5, and the degree of wear of Examples 10-12 during the friction process of 1100-4500 times is the same as that of Example 5, indicating that when mussel mucin, polyglutamic acid, and chitosan derivatives are used, they all have synergistic antibacterial properties and further improve the antibacterial properties of the antibacterial fabric, while allowing the antibacterial fabric to maintain good tear resistance.

[0066] Combining Example 11 and Example 15 and Table 2, it can be seen that the increase in the antibacterial rate of Example 15 is higher than that of Example 11, and the degree of wear of Example 15 during the friction process of 1100-4500 times is the same as that of Example 11, indicating that when sulfonated chitosan and methacryloyl chitosan are used, a synergistic antibacterial effect is achieved, and they cooperate with mussel mucin, polyglutamic acid, etc., so that the antibacterial yarn treated with the toughening agent may break or wear, so that the antibacterial fabric has both better antibacterial and wear resistance.

[0067] It can be seen from the structure of Example 4 and Examples 16-20 in combination with Table 2 that the degree of wear of Examples 16-20 during the friction process of 1100-4500 times is as serious as that of Example 4, and the increase in antibacterial rate is lower than that of Example 4, indicating that when 3-methacryloyloxy-2-hydroxypropoxy)propyl bis(trimethylsiloxy)methyl, methoxypolyethylene glycol acrylate, methacryloylethyl sulfobetaine, and antibacterial thickener are compounded and act together, the toughened antibacterial treatment agent obtained has a better toughening effect on the antibacterial yarn, reducing the possibility of breakage, wear, bacterial growth, pilling, etc. caused by the antibacterial fabric being eroded by sweat.

[0068] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.

Claims

1. An antibacterial fabric containing seaweed fiber, characterized in that: The antibacterial yarn is knitted, wherein the antibacterial yarn is composed of 85-92% by mass of regenerated cellulose fiber and 8-15% by mass of seaweed fiber, and the antibacterial yarn has a count of 30-40.

2. The antibacterial fabric containing seaweed fiber according to claim 1, characterized in that: The weight of the antibacterial fabric is 100-150g / m 3 .

3. The antibacterial fabric containing seaweed fiber according to claim 1, characterized in that: The antibacterial yarn is treated with a toughening agent, and the toughening agent is composed of the following raw materials in parts by weight: 20-30 parts water 1-5 parts of environmentally friendly organic solvent Antibacterial viscosity enhancer 0.8-1.7 parts Emulsifier 0.5-1 part Ammonium persulfate 0.1-0.3 parts Methoxy polyethylene glycol acrylate 0.01-0.08 parts Methacryloylethyl sulfobetaine 0.5-1.8 parts 0.1-0.5 parts of (3-methacryloyloxy-2-hydroxypropoxy)propylbis(trimethylsilyloxy)methyl 4. The antibacterial fabric containing seaweed fiber according to claim 3, characterized in that: The antibacterial viscosity enhancer is composed of one or more of mussel mucin, polyglutamic acid and chitosan derivatives.

5. The antibacterial fabric containing seaweed fiber according to claim 4, characterized in that: The antibacterial viscosity enhancer consists of mussel mucin, polyglutamic acid and chitosan derivatives.

6. The antibacterial fabric containing seaweed fiber according to claim 5, characterized in that: The weight ratio of the mussel mucin, polyglutamic acid and chitosan derivative is (3-8):3:(2-7).

7. The antibacterial fabric containing seaweed fiber according to claim 6, characterized in that: The chitosan derivative is sulfonated chitosan and / or methacrylylated chitosan.

8. The antibacterial fabric containing seaweed fiber according to claim 3, characterized in that: The emulsifier is one or more of cocamidopropyl betaine, OP-10, OP-20, and sodium lauryl sulfate.

9. The antibacterial fabric containing seaweed fiber according to claim 3, characterized in that: The environmentally friendly organic solvent is anhydrous ethanol and / or dipropylene glycol dimethyl ether.

10. A method for preparing an antibacterial fabric containing seaweed fiber according to any one of claims 1 to 9, characterized in that: The following steps are involved: The seaweed fiber and the regenerated cellulose fiber are twisted to obtain antibacterial yarn; the antibacterial yarn is then knitted to obtain antibacterial fabric.

Citation Information

Patent Citations

  • Method for producing antibacterial seaweed fabric

    CN105463672A

  • Knitted fabric and manufacturing method thereof

    CN111304812A

  • Antibacterial and anti-mite alginate fiber fabric and preparation process thereof

    CN113265755A