Cationic modifier for cotton fabric and preparation method thereof

The stability of quaternary ammonium salt modifiers and baicalin were solved by supporting the combination of dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride and aqueous silk peptide solution in nano SiO2 carrier. The problem of insufficient dye color fastness has achieved more lasting dyeing effect and antibacterial properties.

CN118979387APending Publication Date: 2024-11-19YUNFU HAIXING ENVIRONMENTAL PROTECTION TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411211261.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The application of quaternary ammonium salt cationic modifiers on cotton fabrics has insufficient heat resistance and chemical stability, insufficient efficacy, poor color fastness of baicalin natural dyes, and insufficient color and fatigue of soap washing.

Method used

A nano-SiO2 particle carrier is used to carry dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride and silk peptide aqueous solution, combined with malic acid aqueous solution, to prepare a cationic modification for cotton fabrics. The agent can improve the chemical stability and antibacterial properties of the modifier through specific process treatment, and improve the color fastness of baicalin dyes.

Benefits of technology

It significantly improves the heat resistance and chemical stability of quaternary ammonium salt cationic modifiers, extends its action time, improves the soap washing and color fastness of baicalin dyes, enhances the antibacterial properties, and improves the Anti-fouling and self-cleaning performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005020364550000131
    Figure BDA0005020364550000131
  • Figure BDA0005020364550000132
    Figure BDA0005020364550000132
  • Figure BDA0005020364550000142
    Figure BDA0005020364550000142
Patent Text Reader

Abstract

The invention belongs to the technical field of preparation of cationic modifiers, and particularly relates to an efficient cationic modifier component for cotton fabrics and a preparation method of the efficient cationic modifier component. The efficient cationic modifier for the cotton fabric comprises 6-9 g of nano SiO2 particles, 3-5 mL of dimethyl octadecyl [3-(trimethoxysilyl) propyl] ammonium chloride, 100-150 mL of methylbenzene, 45-55 mL of a silk peptide aqueous solution with the concentration of 3.5 g / 100 mL and 15-25 mL of a malic acid aqueous solution with the concentration of 2 g / 100 mL. The efficient cationic modifier for the cotton fabric has high heat resistance and chemical stability and is not prone to loss, and the chemical stability of the ammonium salt cationic modifier is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of dyeing and finishing, and in particular relates to a cationic modifier for cotton fabric and a preparation method thereof. Background Art

[0002] The application of cationic modifiers in cotton fabric treatment is mainly to enhance the fiber's adsorption capacity for dyes by introducing positively charged groups, thereby improving the dyeing effect and dye fastness. This type of modifier usually refers to special cationic polymers. After reacting with cellulose fibers, they can make the fibers cationic and significantly improve the dyeing rate of active and direct dyes on the fibers. The mechanism of action of cationic modifiers involves the situation that the fibers are charged in the dye solution, reducing the electrostatic repulsion between the dye and the fiber, and improving the dyeing rate and dyeing quality of the dye. In the specific process flow, the cotton fabric needs to be wetted first, then treated with cationic modifiers, then the pH value of the dye bath is adjusted with soda ash, the temperature is gradually increased, and finally washed with water. The use of cationic modifiers can overcome the repulsion of the negatively charged fabric to the negatively charged latex particles and improve the impregnation effect. In addition, cationic modifiers can also improve the feel of paint-dyed fabrics, reduce or eliminate the need for the use of adhesives, and maintain good color fastness.

[0003] The types of cationic modifiers mainly include quaternary ammonium salts, fatty amines, ureas and acetals. These modifiers vary in their respective properties and application areas and are widely used to improve the performance and stability of products.

[0004] However, although the application of quaternary ammonium salt cationic modifiers on cotton fabrics can significantly improve the dyeing performance, increase the dyeing rate and color fastness of natural dyes on cotton fabrics, there may also be some disadvantages in practical applications. Specific disadvantages may include:

[0005] Quaternary ammonium salt modifiers have certain negative impacts on the environment. Their heat resistance and chemical stability are not high enough, their effectiveness is not long-lasting, and they are easily lost.

[0006] On the other hand, for cotton fabrics, baicalin natural dye can dye silk fabrics into light yellow, while giving them excellent antioxidant, antibacterial and anti-ultraviolet functions. However, baicalin natural dye has a slightly poor soap color resistance, especially the color change level.

[0007] The cotton fabric cationic modifier of the present application aims to solve the technical problem that the quaternary ammonium salt modifier is not long-lasting and easily lost, and on the other hand, solves the poor color fastness of baicalin natural dye. Summary of the invention

[0008] One object of the present invention is to provide a cationic modifier for cotton fabrics, which can improve the chemical stability of quaternary ammonium salt modifiers and increase the duration of their effectiveness. On the other hand, the cationic modifier has the effect of improving the soap color labor of baicalin natural dyes.

[0009] Another object of the present invention is to provide a method for preparing a cationic modifier for cotton fabric, which can be used to prepare the cationic modifier for cotton fabric.

[0010] The invention also discloses a method for using the cationic modifier for cotton fabric.

[0011] Accordingly, the first aspect of the present invention is to provide a cationic modifier for cotton fabric, which contains the following components:

[0012] 6~9g nano-SiO 2 particles, 3-5 mL of dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride, 100-150 mL of toluene, 45-55 mL of a silk peptide aqueous solution, the concentration of the silk peptide aqueous solution is 3.5 g / 100 mL, and 15-25 mL of a malic acid aqueous solution, the concentration of the malic acid aqueous solution is 2 g / 100 mL.

[0013] Preferably, the nano-SiO 2 The mass of the particle is 7 g.

[0014] Preferably, the volume of dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride is 3.5 mL.

[0015] Preferably, the volume of toluene is 125 mL.

[0016] Preferably, the volume of the silk peptide aqueous solution is 50 mL.

[0017] Preferably, the malic acid aqueous solution is 20 mL.

[0018] Preferably, the preparation method of the silk peptide aqueous solution is as follows: waste or raw silk is used as raw material, the silk can be selected from mulberry silk or tussah silk, first washed, dried, cut, placed in a 3% by mass barium hydroxide aqueous solution, heated to 90-95 degrees Celsius, and the silk fibers are hydrolyzed, and this temperature is maintained for 5-6 hours to complete the hydrolysis. After the hydrolysis is completed, dilute sulfuric acid is used to neutralize to a pH of 6-7, and barium sulfate impurities are filtered to obtain a silk peptide solution, which is concentrated and dried to obtain a silk peptide solid, and a silk peptide solution of corresponding concentration is prepared as needed.

[0019] The second aspect of the present invention is to provide a method for preparing a cationic modifier for cotton fabric;

[0020] S1, accurately weigh nano-SiO 2Particles, dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride, toluene for later use, silk peptide aqueous solution, malic acid aqueous solution for later use;

[0021] S2, add weighed nano-SiO 2 Particles, add weighed toluene, stir for 30-45 minutes, mix evenly;

[0022] S3, maintaining the stirring state, and adding weighed dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride to the conical flask, raising the reaction temperature to 85 degrees Celsius to 90 degrees Celsius, and stopping the reaction after 2 to 4 hours, filtering the obtained reaction mixture, and placing the product obtained after filtration in a vacuum drying oven to dry to constant weight to obtain dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride modified nano-SiO 2 Particles, nano-SiO2 modified by dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride 2 The particles are recorded as product A;

[0023] S4, soaking the dried product A in a weighed silk peptide aqueous solution, adding a weighed malic acid aqueous solution, stirring continuously for 1 to 2 hours, and maintaining the temperature at 40 to 50 degrees Celsius during stirring, filtering the obtained reaction mixture, placing the product obtained after filtration in a vacuum drying oven and drying to constant weight to obtain product B, which is a cationic modifier for cotton fabrics.

[0024] Preferably, the stirring time in S2 is 35 min.

[0025] Preferably, the reaction temperature in S3 is 88 degrees Celsius and the reaction time is 3 hours.

[0026] Preferably, the stirring time in S4 is 1 hour, and the temperature is maintained at 50 degrees Celsius during the stirring process.

[0027] The third aspect of the present invention is to provide a method for using a cationic modifier for cotton fabrics.

[0028] Before using baicalin to dye cotton fabric, a certain mass of the prepared cationic modifier for cotton fabric and a 50% by mass ethanol aqueous solution are taken and placed in a beaker to prepare a dispersion of the cationic modifier for cotton fabric with a mass fraction of 0.5% to 3%, the dispersion is magnetically stirred for 20 minutes to 30 minutes for standby use, the dispersion is sprayed on the surface of the cotton fabric at a distance of 20 cm from the surface of the fabric, and after the spraying is uniform, the cotton fabric is baked at 80°C for 25 to 35 minutes to obtain the cotton fabric treated with the cationic modifier, and then the treated cotton fabric is dyed with baicalin.

[0029] Preferably, the mass fraction of the dispersion is 3%.

[0030] Preferably, the time for magnetic stirring of the dispersion is 25 min.

[0031] Preferably, the cotton fabric is baked at 80° C. for 30 minutes.

[0032] Compared with the prior art, the beneficial technical effects of the present invention are:

[0033] (1) The present invention loads the quaternary ammonium salt cationic modifier on the nano-SiO 2 On the other hand, it improves its heat resistance and chemical stability, and it is not easy to lose, which improves the chemical stability of the ammonium salt cationic modifier;

[0034] (2) Nano-SiO 2 At the same time, it provides loading sites for silk peptides. The cotton fabrics treated with silk peptides improve the soap color labor of baicalin natural dyes and improve their color stability during the washing process. 2 To a certain extent, the silk peptide is protected to avoid complete ineffectiveness of the silk peptide in subsequent drying and daily use of cotton fabrics, which leads to decreased color fastness of dyeing, that is, the problem of clothes fading.

[0035] (3) After the above treatment, the antifouling and self-cleaning properties of the cotton fabric using the cationic modifier are improved accordingly.

[0036] (4) Since both the quaternary ammonium salt cationic modifier and baicalin have antibacterial effects, the cotton fabric treated with the quaternary ammonium salt cationic modifier has better antibacterial properties and longer-lasting antibacterial properties. DETAILED DESCRIPTION

[0037] In order to more fully understand the technical content of the present invention, the present invention will be further introduced and illustrated in conjunction with specific embodiments below; obviously, the embodiments described below are only part of the embodiments of the present invention, rather than all of the embodiments; based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making creative work are within the scope of protection of the present invention.

[0038] Example 1

[0039] A cationic modifier for cotton fabric, comprising the following components:

[0040] 7g Nano-SiO 2particles, 3.5 mL of dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride, 125 mL of toluene, 50 mL of silk peptide aqueous solution, the concentration of the silk peptide aqueous solution is 3.5 g / 100 mL, 20 mL of malic acid aqueous solution, the concentration of the malic acid aqueous solution is 2 g / 100 mL;

[0041] The preparation method of the silk peptide aqueous solution is as follows: using waste mulberry silk as a raw material, first washing, drying, cutting, placing in 100 mL of a 3% by mass barium hydroxide aqueous solution, heating to 90 degrees Celsius, hydrolyzing the silk fibers, maintaining this temperature for 5 hours to complete the hydrolysis, and after the hydrolysis is completed, using dilute sulfuric acid to neutralize to pH 7, filtering barium sulfate impurities to obtain a silk peptide solution, concentrating and drying to obtain a silk peptide solid, and preparing a silk peptide solution of corresponding concentration as needed;

[0042] The preparation process of the cationic modifier for cotton fabric comprises:

[0043] S1, accurately weigh nano-SiO 2 Particles, dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride, toluene for later use, silk peptide aqueous solution, malic acid aqueous solution for later use;

[0044] S2, add weighed nano-SiO 2 Particles, add weighed toluene, stir for 35 minutes, mix well;

[0045] S3, maintaining the stirring state, and adding weighed dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride to the conical flask, raising the reaction temperature to 85 degrees Celsius, and stopping the reaction after 3 hours, filtering the obtained reaction mixture, and placing the product obtained after filtration in a vacuum drying oven to dry to constant weight to obtain dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride modified nano-SiO 2 Particles, nano-SiO2 modified by dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride 2 The particles are recorded as product A;

[0046] S4, soaking the dried product A in a weighed silk peptide aqueous solution, adding a weighed malic acid aqueous solution, stirring for 1 hour, and maintaining the temperature at 50 degrees Celsius during the stirring process, filtering the obtained reaction mixture, placing the product obtained after filtration in a vacuum drying oven and drying to constant weight to obtain product B, which is a cationic modifier for cotton fabrics;

[0047] The method for using the cationic modifier for cotton fabric comprises:

[0048] Before using baicalin to dye cotton fabric, a certain mass of the prepared cationic modifier for cotton fabric and a 50% by mass ethanol aqueous solution are taken and placed in a beaker to prepare a dispersion of the cationic modifier for cotton fabric with a mass fraction of 3%, the dispersion is magnetically stirred for 25 minutes, and the dispersion is sprayed on the surface of the cotton fabric at a distance of 20 cm from the surface of the fabric. After spraying evenly, the cotton fabric is baked at 80°C for 30 minutes to obtain cotton fabric treated with the cationic modifier, and then the treated cotton fabric is dyed with baicalin.

[0049] Example 2

[0050] A cationic modifier for cotton fabric, comprising the following components:

[0051] 8g nano-SiO 2 particles, 4 mL of dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride, 130 mL of toluene, 48 mL of silk peptide aqueous solution, the concentration of the silk peptide aqueous solution is 3.5 g / 100 mL, 18 mL of malic acid aqueous solution, the concentration of the malic acid aqueous solution is 2 g / 100 mL;

[0052] The preparation method of the silk peptide aqueous solution is as follows: using waste mulberry silk as a raw material, first washing, drying, cutting, placing in 100 mL of a 3% by mass barium hydroxide aqueous solution, heating to 90 degrees Celsius, hydrolyzing the silk fibers, maintaining this temperature for 5 hours to complete the hydrolysis, and after the hydrolysis is completed, using dilute sulfuric acid to neutralize to a pH of 6.5, filtering barium sulfate impurities to obtain a silk peptide solution, concentrating and drying to obtain a silk peptide solid, and preparing a silk peptide solution of corresponding concentration as needed;

[0053] The preparation process of the cationic modifier for cotton fabric comprises:

[0054] S1, accurately weigh nano-SiO 2 Particles, dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride, toluene for later use, silk peptide aqueous solution, malic acid aqueous solution for later use;

[0055] S2, add weighed nano-SiO 2 Particles, add weighed toluene, stir for 35 minutes, mix well;

[0056] S3, maintaining the stirring state, and adding weighed dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride to the conical flask, raising the reaction temperature to 90 degrees Celsius, and stopping the reaction after 3 hours, filtering the obtained reaction mixture, and placing the product obtained after filtration in a vacuum drying oven to dry to constant weight to obtain dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride modified nano-SiO2 Particles, nano-SiO2 modified by dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride 2 The particles are recorded as product A;

[0057] S4, soaking the dried product A in a weighed silk peptide aqueous solution, adding a weighed malic acid aqueous solution, stirring for 1 hour, and maintaining the temperature at 45 degrees Celsius during the stirring process, filtering the obtained reaction mixture, placing the product obtained after filtration in a vacuum drying oven and drying to constant weight to obtain product B, which is a cationic modifier for cotton fabrics;

[0058] The method for using the cationic modifier for cotton fabric comprises:

[0059] Before using baicalin to dye cotton fabric, a certain mass of the prepared cationic modifier for cotton fabric and a 50% by mass ethanol aqueous solution are taken and placed in a beaker to prepare a dispersion of the cationic modifier for cotton fabric with a mass fraction of 3%, the dispersion is magnetically stirred for 25 minutes, and the dispersion is sprayed on the surface of the cotton fabric at a distance of 20 cm from the surface of the fabric. After spraying evenly, the cotton fabric is baked at 80°C for 30 minutes to obtain cotton fabric treated with the cationic modifier, and then the treated cotton fabric is dyed with baicalin.

[0060] Example 3

[0061] A cationic modifier for cotton fabric, comprising the following components:

[0062] 9g Nano-SiO 2 particles, 5 mL of dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride, 100 mL of toluene, 55 mL of silk peptide aqueous solution, the concentration of the silk peptide aqueous solution is 3.5 g / 100 mL, 20 mL of malic acid aqueous solution, the concentration of the malic acid aqueous solution is 2 g / 100 mL;

[0063] The preparation method of the silk peptide aqueous solution is as follows: using waste mulberry silk as a raw material, first washing, drying, cutting, placing in 100 mL of a 3% by mass barium hydroxide aqueous solution, heating to 90 degrees Celsius, hydrolyzing the silk fibers, maintaining this temperature for 5 hours to complete the hydrolysis, and after the hydrolysis is completed, using dilute sulfuric acid to neutralize to pH 7, filtering barium sulfate impurities to obtain a silk peptide solution, concentrating and drying to obtain a silk peptide solid, and preparing a silk peptide solution of corresponding concentration as needed;

[0064] The preparation process of the cationic modifier for cotton fabric comprises:

[0065] S1, accurately weigh nano-SiO 2Particles, dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride, toluene for later use, silk peptide aqueous solution, malic acid aqueous solution for later use;

[0066] S2, add weighed nano-SiO 2 Particles, add weighed toluene, stir for 35 minutes, mix well;

[0067] S3, maintaining the stirring state, and adding weighed dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride to the conical flask, raising the reaction temperature to 85 degrees Celsius, and stopping the reaction after 4 hours, filtering the obtained reaction mixture, and placing the product obtained after filtration in a vacuum drying oven to dry to constant weight to obtain dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride modified nano-SiO 2 Particles, nano-SiO2 modified by dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride 2 The particles are recorded as product A;

[0068] S4, soaking the dried product A in a weighed silk peptide aqueous solution, adding a weighed malic acid aqueous solution, stirring for 2 hours, and maintaining the temperature at 50 degrees Celsius during the stirring process, filtering the obtained reaction mixture, placing the product obtained after filtration in a vacuum drying oven and drying to constant weight to obtain product B, which is a cationic modifier for cotton fabrics;

[0069] The method for using the cationic modifier for cotton fabric comprises:

[0070] Before using baicalin to dye cotton fabric, a certain mass of the prepared cationic modifier for cotton fabric and a 50% by mass ethanol aqueous solution are taken and placed in a beaker to prepare a dispersion of the cationic modifier for cotton fabric with a mass fraction of 3%, the dispersion is magnetically stirred for 25 minutes, and the dispersion is sprayed on the surface of the cotton fabric at a distance of 20 cm from the surface of the fabric. After spraying evenly, the cotton fabric is baked at 80°C for 30 minutes to obtain cotton fabric treated with the cationic modifier, and then the treated cotton fabric is dyed with baicalin.

[0071] Comparative Example 1

[0072] Compared with Example 1, the only difference is:

[0073] The preparation process of the cationic modifier for cotton fabric does not include step S4, and the method for using the cationic modifier for cotton fabric is replaced by:

[0074] Before using baicalin to dye cotton fabric, a certain mass of the prepared product A and a 50% ethanol aqueous solution are taken and placed in a beaker to prepare a dispersion of product A with a mass fraction of 3%. The dispersion is magnetically stirred for 25 minutes for standby use. The dispersion is sprayed on the surface of the cotton fabric at a distance of 20 cm from the fabric surface, and 55 mL of a 3.5 g / 100 mL silk peptide aqueous solution and 20 mL of a 2 g / 100 mL malic acid aqueous solution are evenly sprayed on the surface of the cotton fabric. After spraying evenly, the cotton fabric is baked at 80°C for 30 minutes to obtain a cotton fabric treated with a cationic modifier, and then the treated cotton fabric is dyed with baicalin.

[0075] Comparative Example 2

[0076] Compared with Example 1, the only difference is:

[0077] The method of using the cationic modifier for cotton fabric is replaced by:

[0078] Before using black tea to dye cotton fabric, a certain mass of the prepared cationic modifier for cotton fabric and a 50% by mass ethanol aqueous solution are taken and placed in a beaker to prepare a dispersion of the cationic modifier for cotton fabric with a mass fraction of 3%, the dispersion is magnetically stirred for 25 minutes for standby use, the dispersion is sprayed on the surface of the cotton fabric at a distance of 20 cm from the surface of the fabric, and after spraying evenly, the cotton fabric is baked at 80°C for 30 minutes to obtain cotton fabric treated with the cationic modifier, and then the treated cotton fabric is dyed with black tea.

[0079] Comparative Example 3

[0080] Compared with Example 2, the only difference is:

[0081] The preparation process of the cationic modifier for cotton fabric is replaced by:

[0082] S1, accurately weigh nano-SiO 2 Particles, dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride, toluene for later use, silk peptide aqueous solution, malic acid aqueous solution for later use;

[0083] S2, add weighed nano-SiO 2 Particles, add weighed toluene, stir for 35 minutes, mix well;

[0084] S3, filtering the substance obtained in S2, and placing the product obtained after filtration in a vacuum drying oven to dry to constant weight, to obtain product C;

[0085] S4, soaking the dried product C in a weighed silk peptide aqueous solution, adding a weighed malic acid aqueous solution, stirring for 1 hour, and maintaining the temperature at 45 degrees Celsius during the stirring process, filtering the obtained reaction mixture, and placing the product obtained after filtration in a vacuum drying oven to dry to constant weight to obtain product B', which is a modifier for cotton fabrics;

[0086] The method for using the cationic modifier for cotton fabric comprises:

[0087] Before using baicalin to dye cotton fabric, a certain mass of the prepared product B' and a 50% ethanol aqueous solution by mass are taken and placed in a beaker to prepare a dispersion of a modifier for cotton fabric with a mass fraction of 3%. The dispersion is magnetically stirred for 25 minutes for later use. The dispersion is sprayed on the surface of the cotton fabric at a distance of 20 cm from the surface of the fabric, and 5 mL of dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride is sprayed. After spraying evenly, the cotton fabric is baked at 80°C for 30 minutes to obtain a cotton fabric treated with a modifier. The treated cotton fabric is then dyed with baicalin.

[0088] Comparative Example 4

[0089] Compared with Example 3, the only difference is:

[0090] The method of using the cationic modifier for cotton fabric is replaced by:

[0091] Before using madder to dye cotton fabric, a certain mass of the prepared cationic modifier for cotton fabric and a 50% by mass ethanol aqueous solution are taken and placed in a beaker to prepare a dispersion of the cationic modifier for cotton fabric with a mass fraction of 3%, the dispersion is magnetically stirred for 25 minutes, and the dispersion is sprayed on the surface of the cotton fabric at a distance of 20 cm from the surface of the fabric. After spraying evenly, the cotton fabric is baked at 80°C for 30 minutes to obtain cotton fabric treated with the cationic modifier, and then the treated cotton fabric is dyed with madder.

[0092] After dyeing, the K / S values ​​of the dyed samples of Examples 1 to 3 and Comparative Examples 1 to 4 were measured, and the results are shown in the following table:

[0093] Table 1 K / S value of dyed fabrics

[0094] Dyeing conditions K / S value Direct dyeing K / S value Example 1 3.205 1.021 Example 2 3.217 0.989 Example 3 3.198 1.018 Comparative Example 1 3.521 1.058 Comparative Example 2 2.695 0.990 Comparative Example 3 3.014 1.002 Comparative Example 4 2.475 0.905

[0095] As can be seen from the table above, before using the modifier, the dyeing rate of natural dyes was very low, but after being treated with the modifier, the dyeing rate increased. Comparative Example 1 proves that the dyeing effect of directly using silk peptide for spraying is better. Comparative Examples 2 and 4 prove that silk peptide has a stronger degree of deepening baicalin than black tea and madder. This may be due to the -NH 2 , -OH, etc. can undergo cross-linking reaction with cotton fiber through citric acid, and the cotton fiber after the reaction is more easily combined with the keto group on baicalin. The result of comparative example 3 may be due to the fact that dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride is not loaded on nano-SiO 2 On the particles, during the baking process of cotton fabric at 80°C for 30 minutes, a very small part of it was lost, resulting in a decrease in its effect on improving dyeing performance.

[0096] After dyeing, the color fastness of Examples 1 to 3 and Comparative Examples 1 to 4 was measured, and the results are shown in the following table:

[0097] Table 2 Color fastness of dyed fabrics

[0098]

[0099] Table 3 Color fastness of dyed fabrics directly dyed (without using any modifier, direct dyeing with silk peptide)

[0100]

[0101]

[0102] From Table 2-3, it can be seen that the color fastness of cotton fabric to baicalin is improved by using cationic modifier, but for other dyes, such as black tea and madder, the soaping and rubbing fastness of the dyed fabric decreases slightly after finishing with cationic modifier containing silk peptide. For Comparative Examples 1 and 3, since they are not loaded, part of the silk peptide and cationic modifier are seriously lost, resulting in reduced color fastness.

[0103] After dyeing, two circular cotton fabrics with a radius of 1 cm were taken and placed in potato dextrose agar medium respectively, and Aspergillus niger and Gloeophyllum trabeum were inoculated in the medium respectively. After a period of time (7 days), the radius of the inhibition zone was measured.

[0104] After dyeing, the cotton fabric was placed in a high temperature and high humidity environment for one month, with a temperature of 50 degrees Celsius and a humidity of 80%. Then, two pieces of treated circular cotton fabric with a radius of 1 cm were taken, cooled, and placed in potato dextrose agar medium respectively, and Aspergillus niger and Gloeophyllum trab eum were inoculated in the medium respectively. After a period of time (7 days), the radius of the inhibition zone was measured.

[0105] Table 4 Antibacterial properties of dyed fabrics

[0106]

[0107]

[0108] From the above table, it can be seen that by comparing Comparative Example 1 with Example 1, and by comparing Comparative Example 3 with Example 2, nano-SiO 2 It provides a relatively stable environment for silk peptides and quaternary ammonium salts, reduces the impact of the external environment on the two, and ensures the antibacterial durability of silk peptides and quaternary ammonium salts in harsh environments; compared with comparative examples 2 and 4, and embodiments 1-3, it can be seen that the antibacterial properties of black tea and madder are poorer than baicalin, which also proves that the natural substance baicalin has a certain antibacterial effect.

[0109] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.

Claims

1. A cationic modifier for cotton fabric, characterized in that: Contains the following components: 6-9 g of nano-SiO2 particles, 3-5 mL of dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride, 100-150 mL of toluene, 45-55 mL of silk peptide aqueous solution, the concentration of the silk peptide aqueous solution is 3.5 g / 100 mL, 15-25 mL of malic acid aqueous solution, the concentration of the malic acid aqueous solution is 2 g / 100 mL.

2. According to the cationic modifier for cotton fabrics according to claim 1, the mass of the nano-SiO2 particles is 7g; the volume of the dimethyloctadecyl [3- (trimethoxysilyl) propyl] ammonium chloride is 3.5mL; the volume of the toluene is 125mL; the volume of the silk peptide aqueous solution is 50mL; and the malic acid aqueous solution is 20mL.

3. The cationic modifier for cotton fabric according to claim 1, wherein the preparation method of the silk peptide aqueous solution is as follows: waste silk or raw silk is used as raw material, and the silk can be selected from mulberry silk or tussah silk, is first washed, dried, and cut, and then placed in a 3% by mass barium hydroxide aqueous solution, heated to 90-95 degrees Celsius, and the silk fiber is hydrolyzed, and this temperature is maintained for 5-6 hours to complete the hydrolysis. After the hydrolysis is completed, dilute sulfuric acid is used to neutralize to a pH of 6-7, and after filtering out barium sulfate impurities, a silk peptide solution is obtained, which is concentrated and dried to obtain a silk peptide solid, and a silk peptide solution of corresponding concentration is prepared as required.

4. A method for preparing a cationic modifier for cotton fabric, characterized in that: The following steps are involved: S1, accurately weigh nano-SiO2 particles, dimethyl octadecyl [3-(trimethoxysilyl) propyl] ammonium chloride, toluene, silk peptide aqueous solution, and malic acid aqueous solution for use, the nano-SiO2 particles are 7 g, the volume of dimethyl octadecyl [3-(trimethoxysilyl) propyl] ammonium chloride is 3.5 mL, the volume of toluene is 125 mL, the volume of silk peptide aqueous solution is 50 mL, the concentration of silk peptide aqueous solution is 3.5 g / 100 mL, the malic acid aqueous solution is 20 mL, and the concentration of malic acid aqueous solution is 2 g / 100 mL; S2, add weighed nano-SiO2 particles and weighed toluene into a conical flask, stir for 30 to 45 minutes, and mix well; S3, maintaining the stirring state, and adding weighed dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride to the conical flask, raising the reaction temperature to 85 degrees Celsius to 90 degrees Celsius, and stopping the reaction after 2 to 4 hours, filtering the obtained reaction mixture, and placing the product obtained after filtration in a vacuum drying oven to dry to constant weight to obtain dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride modified nano-SiO2 particles, dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride modified nano-SiO2 particles are recorded as product A; S4, soaking product A in a weighed silk peptide aqueous solution, adding a weighed malic acid aqueous solution, stirring continuously for 1 to 2 hours, and maintaining the temperature at 40 to 50 degrees Celsius during stirring, filtering the obtained reaction mixture, placing the product obtained after filtration in a vacuum drying oven and drying to constant weight to obtain product B, which is a cationic modifier for cotton fabrics.

5. The method for preparing a cationic modifier for cotton fabric according to claim 4, wherein the stirring time in S2 is specifically 35 minutes; and the reaction temperature in S3 is increased to 88 degrees Celsius, and the reaction time is 3 hours.

6. The method for preparing a cationic modifier for cotton fabric according to claim 4, wherein the continuous stirring time in S4 is 1 hour, and the temperature is maintained at 50 degrees Celsius during the stirring process.

7. A method for using a cationic modifier for cotton fabric, characterized in that: Before using baicalin to dye cotton fabric, a certain mass of the prepared cationic modifier for cotton fabric and a 50% by mass ethanol aqueous solution are taken and placed in a beaker to prepare a dispersion of the cationic modifier for cotton fabric, wherein the cationic modifier for cotton fabric accounts for 0.5% to 3% of the total mass of the dispersion, the dispersion is magnetically stirred for 20 minutes to 30 minutes for standby use, the dispersion is sprayed on the surface of the cotton fabric at a distance of 20 cm from the surface of the fabric, and after the spraying is uniform, the cotton fabric is baked at 80° C. for 25 to 35 minutes to obtain cotton fabric treated with the cationic modifier, and then the treated cotton fabric is dyed with baicalin.

8. The method for using the cationic modifier for cotton fabric according to claim 7, wherein in the cationic modifier dispersion for cotton fabric, the cationic modifier for cotton fabric accounts for 3% of the total mass of the dispersion. 9 . The method for using the cationic modifier for cotton fabric according to claim 7 , wherein the time for magnetic stirring of the dispersion liquid is 25 minutes.

10. The method for using the cationic modifier for cotton fabric according to claim 7, wherein the cotton fabric is baked at 80°C for 30 minutes.