Loudspeaker box wrapping cloth with waterproof and dustproof effects and attaching method thereof

By applying superhydrophobic modified nylon fiber membrane on the speaker bag cloth, combined with the combination technology of fluorine-modified silicone oil and oleic acid-modified nano-silicon dioxide, an efficient hydrophobic film layer is formed, which solves the insufficient waterproof and dustproof performance of the speaker bag cloth. The problem of this achieves extremely high water contact angle and stable anti-pollution performance.

CN118979391APending Publication Date: 2024-11-19GUANGZHOU DUSHANG ELECTRONIC MATERIAL MFG CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411060441.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing speaker cloth has poor waterproof, dust-proof and anti-pollution performance, making it difficult to meet the needs of efficient protection.

Method used

Using superhydrophobic modified nylon fiber membrane, a film layer with strong hydrophobicity and nano-convex structure is formed by spraying the nylon fiber membrane with fluorine-modified silicone oil finishing agent and oleic acid modified nanosilicon dioxide, and then heat melting The adhesive film is hot pressed and bonded to the audio cover.

Benefits of technology

The waterproof, dust-proof and pollution-proof performance of the speaker bag cloth is significantly improved, the water contact angle reaches 158.2°, and the performance remains stable after multiple washes, without significant decline.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004978305030000031
    Figure BDA0004978305030000031
  • Figure BDA0004978305030000092
    Figure BDA0004978305030000092
  • Figure FDA0004978305020000011
    Figure FDA0004978305020000011
Patent Text Reader

Abstract

The invention relates to the technical field of loudspeaker box wrapping cloth, and discloses waterproof and dustproof loudspeaker box wrapping cloth and a laminating method thereof.The loudspeaker box wrapping cloth is prepared by compounding a fluorine modified silicone oil finishing agent and oleic acid modified nano-silica to obtain a finishing liquid, and after surface finishing modification is conducted on a nylon fiber membrane, the nylon fiber membrane is subjected to surface modification; a trifluoromethyl and biphenyl hydrophobic structure organic silicon film layer is introduced on the surface of the fiber film and has very strong hydrophobicity, and oleic acid modified nano silicon dioxide is uniformly dispersed on the organic silicon film layer to form a nano micro-convex structure, so that the surface hydrophobicity of the nylon fiber film and the sound equipment wrapping cloth thereof is remarkably improved, the highest water contact angle reaches 154.2 degrees, and the sound equipment wrapping cloth has good sound equipment performance. The super-hydrophobic nylon fiber membrane shows unique super-hydrophobic characteristics, and can endow the nylon fiber membrane and the loudspeaker box wrapping cloth with waterproof, dustproof and anti-pollution properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of speaker cover cloths, and in particular to a speaker cover cloth having waterproof and dustproof functions and a bonding method thereof. Background Art

[0002] Speakers are a common music playing device. Usually, a layer of speaker wrapping cloth is set on the outside of the speaker of the speaker to play the role of waterproof, dustproof and pollution-proof, protecting the speaker and ensuring the sound quality of the speaker. The current speaker wrapping cloth is mainly made of textiles such as nylon fiber and cotton and linen fiber. Among them, nylon fiber has the advantages of high strength, good wear resistance, and high elastic recovery rate, and is widely used. However, nylon fiber-based speaker wrapping cloth does not have super hydrophobic properties, and its waterproof, dustproof and pollution-proof performance is poor.

[0003] Super-hydrophobic material is a new functional material, has good waterproof and anti-pollution performance, and has broad application prospects in self-cleaning anti-pollution, coating, textiles, etc. Organosilicon finishing agent is a common textile finishing agent, can improve the properties such as softness and feel of fiber textiles, and announcement number is CN115467168B discloses a preparation method of a durable super-hydrophobic cotton / nylon 56 blended fabric, nylon 56 / cotton blended fabric is successively processed by the copolymer of dopamine, pentaerythritol tetra-3-mercaptopropionate, tetraallyl silane and methylacetoxypropylmethylsiloxane / dimethylsiloxane, and cotton / nylon 56 blended fabric is obtained to have the multiple functions such as super-hydrophobic self-cleaning. But the preparation technology of the super-hydrophobic nylon blended fabric is more complicated, and after repeated washing, the water contact angle declines by a large margin. Summary of the invention

[0004] The invention solves the problem that the sound box cover cloth has poor waterproof, dustproof and pollution resistance performance.

[0005] The technical solution provided by the present invention is: a method for preparing a speaker cover cloth with waterproof and dustproof effects, wherein the material of the speaker cover cloth is a super-hydrophobic modified nylon fiber membrane;

[0006] The preparation method of super hydrophobic modified nylon fiber membrane is as follows:

[0007] (1) Add hydrogenated silicone oil, isopropanol solution of chloroplatinic acid and inhibitor p-hydroxyanisole to toluene, raise the temperature to 110-125° C. under a nitrogen atmosphere, and add The acrylamide-based fluorine-containing monomer is stirred for reaction for 4-8 hours, the solution is distilled under reduced pressure, washed with methanol, and dried to obtain a fluorine-modified silicone oil finishing agent.

[0008] (2) adding fluorine-modified silicone oil finishing agent, oleic acid-modified nano-silica, and an emulsifier to distilled water, shearing and dispersing, and obtaining a finishing liquid; spraying the finishing liquid onto one side of a nylon fiber membrane using a spray gun, drying at 90-100° C. for 10-20 min, and baking at 170-180° C. for 30-60 s, to obtain a super-hydrophobic modified nylon fiber membrane.

[0009] Furthermore, the mass of the acrylamide-based fluorine-containing monomer in (1) is 3-15% of the mass of the hydrogen-containing silicone oil.

[0010] Furthermore, in (2), the mass of the emulsifier and the oleic acid-modified nano-silica are 6-25% and 40-60% of the mass of the fluorine-modified silicone oil finishing agent, respectively.

[0011] Furthermore, the emulsifier includes OP-10 and fatty alcohol polyoxyethylene ether AEO-9.

[0012] Furthermore, the preparation method of acrylamide-based fluorinated monomer is:

[0013] S1. Add 3-bromo-5-(trifluoromethyl)aniline (CAS registration number is 54962-75-3) and 3-amino-5-trifluoromethylphenylboronic acid pinacol ester (CAS registration number is 510771-54-7) to toluene, add bistriphenylphosphine palladium dichloride and potassium carbonate after stirring, raise the temperature to 75-90°C under nitrogen atmosphere, react for 24-36h, distill the solution under reduced pressure, wash with water and methanol in turn, recrystallize the product with dichloromethane to obtain an aniline fluorine-containing monomer.

[0014] S2. Add aniline fluorinated monomer and triethylamine to dichloromethane at 0-5°C, add acryloyl chloride dropwise after stirring, and then react at room temperature for 12-18 hours. Distill the solution under reduced pressure, wash with water, and recrystallize the product with dichloromethane to obtain acrylamide fluorinated monomer. The reaction formula is as follows:

[0015]

[0016] Furthermore, in S1, the mass of 3-amino-5-trifluoromethylphenylboronic acid pinacol ester is 125-140% of the mass of 3-bromo-5-(trifluoromethyl)aniline.

[0017] Furthermore, in S2, the mass of acryloyl chloride is 60-68% of the mass of the aniline-based fluorinated monomer.

[0018] Furthermore, the method for bonding the waterproof and dustproof speaker cover cloth is as follows: the super-hydrophobic modified nylon fiber membrane is made into a speaker cover cloth of the same size and shape as the speaker cover, and then the side of the fiber membrane that is not sprayed with the finishing liquid is hot-pressed and bonded to the speaker cover by a hot-melt adhesive film (patching). The bonding steps are as follows:

[0019] 1. Install the key sheet: Align the key sheet with the hole position of the lower cover key, then press the key bracket and install it flatly on the mesh cover.

[0020] 2. Glue dispensing: Position the glue dispensing machine in the mold slot, then place the plastic part according to the positioning slot, then press the grid to the bottom of the positioning slot, press the green button to start glue dispensing, and place the glue flat on the card.

[0021] 3. Pasting: Place the mesh foot pads corresponding to the aluminum plate foot pads, press the silicone foot pad mesh piece over the rubber plate and stick it neatly, the foot pad strips should be close to the grooves of the aluminum plate foot pads, and then press the foot pads tightly.

[0022] 4. Laser machine edge cutting: Place the glued sheet on the cutting table according to the positioning groove, make sure the four sides of the glued sheet are flush with the positioning groove of the cutting table, press the green start button to start the laser machine, keep a distance from the laser head during the operation of the laser machine, and clean the cloth edge after the laser head completes the cutting task.

[0023] 5. Gluing the mesh: Cut the edge of the fabric on the glue board, place the mesh facing down, and place the glue board at a 45-degree angle. Put it on the glue roller for gluing, and hold the glued mesh on the glue board with your hands.

[0024] 6. Positioning: The glued surface of the glue board mesh is facing down, the notch of the mesh is consistent with the notch of the lower grid frame, put the glue board into the limiting groove of the positioning fixture, pick up the glue board, turn it 180 degrees and press the glue board to make the lower grid frame stick to the glue board mesh piece.

[0025] 7. Gluing of mesh cloth: The semi-finished product that has been positioned is fixed according to the positioning groove, and two glue plates are placed in the positioning groove in the same direction. The equipment starts to glue and the semi-finished product that has been glued is taken out.

[0026] 8. Arrangement: Press the center of the lower grid with your hand and keep it still. First, gradually adjust the middle mesh around it to make it close to the plastic part, and then adjust the rest of the mesh to make it close to the lower grid. Press the middle of the grid with your thumbs as a support point, press the mesh close to one side of the lower grid and gently flip it off the plastic plate. Press the middle of the grid with your fingers as a support point, adjust the mesh around the lower grid to make it close to the lower grid, and then use your thumb nail to scratch the position of the presser foot.

[0027] 9. Front section inspection: Check whether the foot pads are dislocated, bulged or wrinkled.

[0028] 10. Re-press the foot pad: With the foot pad facing upwards and the notch facing outwards, place the product into the re-pressing mold, start the mesh re-pressing machine, and take out the re-pressed semi-finished product.

[0029] 11. Apply glue: Apply glue on the glue painting position on the edge of the grid frame, and apply glue on the glue painting position on the edge of the mesh cloth.

[0030] 12. Edge wrapping: With the foot pad facing upwards and the notch facing right, place the product into the edge wrapping mold, fix it according to the positioning groove, wrap the edge with the equipment, and take out the product.

[0031] 13. Folding corners: Use a hot air gun to soften the convex corners, and fold the mesh at the convex corners inward into a right angle by hand. Trim the excess mesh at the stacked corners of the edging mesh and along the edge of the mesh frame.

[0032] 14. Re-pressing and edge wrapping: With the foot pad facing downward and the notch facing inward, place the product into the re-pressing mold and start the re-pressing and edge wrapping machine. Take out the re-pressed semi-finished product.

[0033] 15. Perm the corners: Perm the cut convex corners to make them beautiful. There should be no burn marks or fuzzing on the surface after perm. There should be no V-shaped opening when the two sides are closed. The perm position should be flat and there should be no burn brackets. After perm each corner, press the hot position with your hands to make it flat and beautiful.

[0034] 16. Laser drilling: After the semi-finished product has been fully inspected, fix it according to the laser positioning mold, turn on the laser machine, and do not touch the laser head and the optical path while the laser machine is running. Take out the product with holes drilled by the laser machine.

[0035] 17. Install the buttons: Press the power button foot into the correct hole and insert it into place. Press the Bluetooth button foot into the correct hole and insert it into place.

[0036] 18. Hot-melt buttons: With the foot pad facing upward and the buttons facing outward, fix the product according to the positioning mold, hot-melt the buttons with the equipment, and take out the product.

[0037] 19. Full inspection: Check the surface of the product, check that the lines are straight, without bulges, looseness, glue overflow, dirt, or thread ends. Check that the silicone pads are not offset or twisted, that the surrounding mesh is not wrinkled or bulged, and that the silicone pads are not debonded or glue overflowed. Check the finished buttons (press each button twice gently), check that the color is correct, there is no color difference, no pressure damage, no height difference, no looseness, smooth mortise points, no broken legs, flat, no pressure leakage, and check the quality of the mesh cover hemming.

[0038] 20. Packaging: After checking both sides, put the product foot pads outwards, put them together and glue them, put a flat card at the bottom of the carton, and then put the plastic bag into the carton. Put a flat card for each full layer, and seal the carton when it is full. Stick labels according to the corresponding order color, confirm the quantity and label.

[0039] The technical effect of the present invention is that the present invention utilizes acrylamide-based fluorinated monomers to carry out a hydrosilylation reaction on hydrogen-containing silicone oil. The acrylamide-based fluorinated monomers contain two alkenyl groups, which can provide more hydrosilylation reaction sites, thereby increasing the grafting rate of the acrylamide-based fluorinated monomers on the hydrogen-containing silicone oil, thereby introducing more trifluoromethyl and biphenyl hydrophobic structures into the molecular chain of the silicone oil.

[0040] The present invention uses a fluorine-modified silicone oil finishing agent and oleic acid-modified nano-silica to compound and obtain a finishing liquid. After the surface of the nylon fiber membrane is finished and modified, a trifluoromethyl and biphenyl hydrophobic structure organic silicon film layer is introduced on the surface of the fiber membrane, which has strong hydrophobicity, and the oleic acid-modified nano-silica is evenly dispersed in the organic silicon film layer to form a nano-micro-convex structure, which significantly improves the surface hydrophobicity of the nylon fiber membrane and its sound box wrapping cloth, and the water contact angle reaches up to 158.2°, showing a unique super-hydrophobic property, which can give the nylon fiber membrane and its sound box wrapping cloth waterproof, dustproof and anti-pollution properties. In addition, the acrylamide-based fluorine-containing monomer contains more amide bonds, which are grafted into the hydrogen-containing silicone oil, thereby introducing amide bonds in the molecular chain of the fluorine-modified silicone oil finishing agent. After the nylon fiber membrane is finished, the amide bonds of the finishing agent can form a strong chemical interaction force with the amide bonds in the nylon fiber polyamide molecular chain, so that the organic silicon film layer can be firmly attached to the surface of the nylon fiber membrane, which is difficult to wash off, and after washing, the water contact angle does not decrease significantly. DETAILED DESCRIPTION

[0041] The technical solutions in the embodiments of the present application will be described clearly and completely below in conjunction with the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field based on the present application belong to the scope of protection of the present application.

[0042] The hydrogen-containing silicone oil model of the present invention is MY202.

[0043] Hot melt adhesive film, model FJ, made of polyurethane.

[0044] The average particle size of nano-silicon dioxide is 30nm.

[0045] The preparation method of oleic acid modified nano-silica is as follows: add 1g of nano-silica to 30mL of acetone, add 50mg of oleic acid after ultrasonic dispersion, mix well, heat-treat the solution at 120°C until the acetone is completely volatilized, and obtain oleic acid modified nano-silica.

[0046] Example 1

[0047] (1) 2 g of 3-bromo-5-(trifluoromethyl)aniline and 2.5 g of 3-amino-5-trifluoromethylphenylboronic acid pinacol ester were added to 15 mL of toluene, and after stirring, 0.14 g of bistriphenylphosphine palladium dichloride and 4.2 g of potassium carbonate were added. Under a nitrogen atmosphere, the temperature was raised to 75° C. and the reaction was carried out for 36 hours. The solution was distilled under reduced pressure, washed with water and methanol in turn, and the product was recrystallized with dichloromethane to obtain an aniline fluorine-containing monomer.

[0048] (2) At 0°C, 5 g of aniline fluorinated monomer and 4.1 g of triethylamine were added to 50 mL of dichloromethane, and 3.4 g of acryloyl chloride was added dropwise after stirring. The mixture was then reacted at room temperature for 12 h. The solution was distilled under reduced pressure, washed with water, and the product was recrystallized from dichloromethane to obtain an acrylamide fluorinated monomer.

[0049] Example 2

[0050] (1) Add 2 g of 3-bromo-5-(trifluoromethyl)aniline and 2.8 g of 3-amino-5-trifluoromethylphenylboronic acid pinacol ester to 20 mL of toluene, stir, add 0.12 g of bistriphenylphosphine palladium dichloride and 4.6 g of potassium carbonate, heat to 90° C. under nitrogen atmosphere, react for 24 h, distill the solution under reduced pressure, wash with water and methanol in turn, and recrystallize the product with dichloromethane to obtain an aniline fluorine-containing monomer.

[0051] (2) At 5°C, 5 g of aniline fluorinated monomer and 3.5 g of triethylamine were added to 40 mL of dichloromethane, and 3 g of acryloyl chloride was added dropwise after stirring. The mixture was then reacted at room temperature for 18 h. The solution was distilled under reduced pressure, washed with water, and the product was recrystallized from dichloromethane to obtain an acrylamide fluorinated monomer.

[0052] Example 3

[0053] (1) 30 g of hydrogenated silicone oil, 1 mL of an isopropanol solution containing 0.15 mg of chloroplatinic acid, and 4 mg of a polymerization inhibitor, p-hydroxyanisole, were added to 50 mL of toluene. The temperature was raised to 125° C. under a nitrogen atmosphere. 0.9 g of an acrylamide-based fluorinated monomer (prepared in the same manner as in Example 2) was added. The reaction was stirred for 4 h. The solution was distilled under reduced pressure, washed with methanol, and dried to obtain a fluorine-modified silicone oil finishing agent.

[0054] (2) Add 20 g of fluorine-modified silicone oil finishing agent, 1.2 g of oleic acid-modified nano-silica, and 8 g of emulsifier fatty alcohol polyoxyethylene ether AEO-9 to 100 mL of distilled water, shear and disperse, and obtain a finishing liquid; use a spray gun to spray the finishing liquid onto one side of the nylon fiber membrane, dry at 100 ° C for 10 min, and bake at 175 ° C for 60 s to obtain a superhydrophobic modified nylon fiber membrane.

[0055] Example 4

[0056] (1) 30 g of hydrogenated silicone oil, 2 mL of an isopropanol solution containing 0.3 mg of chloroplatinic acid, and 10 mg of a polymerization inhibitor, p-hydroxyanisole, were added to 50 mL of toluene. The temperature was raised to 110° C. under a nitrogen atmosphere. 2 g of an acrylamide-based fluorinated monomer (prepared in the same manner as in Example 2) was added. The mixture was stirred for 8 h. The solution was distilled under reduced pressure, washed with methanol, and dried to obtain a fluorine-modified silicone oil finishing agent.

[0057] (2) Add 20 g of fluorine-modified silicone oil finishing agent, 1.2 g of oleic acid-modified nano-silica, and 11 g of emulsifier OP-10 to 100 mL of distilled water, and shear and disperse to obtain a finishing liquid; use a spray gun to spray the finishing liquid onto one side of the nylon fiber membrane, dry at 100 ° C for 10 min, and bake at 170 ° C for 60 s to obtain a superhydrophobic modified nylon fiber membrane.

[0058] Example 5

[0059] (1) 30 g of hydrogenated silicone oil, 2 mL of an isopropanol solution containing 0.56 mg of chloroplatinic acid, and 16 mg of a polymerization inhibitor, p-hydroxyanisole, were added to 60 mL of toluene. The temperature was raised to 120° C. under a nitrogen atmosphere. 3.2 g of an acrylamide-based fluorinated monomer (prepared in the same manner as in Example 2) was added. The reaction was stirred for 6 h. The solution was distilled under reduced pressure, washed with methanol, and dried to obtain a fluorine-modified silicone oil finishing agent.

[0060] (2) Add 20 g of fluorine-modified silicone oil finishing agent, 1.2 g of oleic acid-modified nano-silica, and 12 g of emulsifier fatty alcohol polyoxyethylene ether AEO-9 to 100 mL of distilled water, shear and disperse, and obtain a finishing liquid; use a spray gun to spray the finishing liquid onto one side of the nylon fiber membrane, dry at 90°C for 15 min, and bake at 180°C for 30 s to obtain a superhydrophobic modified nylon fiber membrane.

[0061] Example 6

[0062] (1) 30 g of hydrogenated silicone oil, 3 mL of an isopropanol solution containing 0.8 mg of chloroplatinic acid, and 22 mg of a polymerization inhibitor, p-hydroxyanisole, were added to 60 mL of toluene. The temperature was raised to 110° C. under a nitrogen atmosphere. 4.5 g of an acrylamide-based fluorinated monomer (prepared in the same manner as in Example 2) was added. The mixture was stirred for 8 h. The solution was distilled under reduced pressure, washed with methanol, and dried to obtain a fluorine-modified silicone oil finishing agent.

[0063] (2) Add 20 g of fluorine-modified silicone oil finishing agent, 1.2 g of oleic acid-modified nano-silica, and 10 g of emulsifier fatty alcohol polyoxyethylene ether AEO-9 to 100 mL of distilled water, shear and disperse, and obtain a finishing liquid; use a spray gun to spray the finishing liquid onto one side of the nylon fiber membrane, dry at 90°C for 20 min, and bake at 180°C for 30 s to obtain a superhydrophobic modified nylon fiber membrane.

[0064] Comparative Example 1 is a nylon fiber membrane without spraying finishing liquid.

[0065] Comparative Example 2

[0066] To 100 mL of distilled water, 20 g of hydrogenated silicone oil, 1.2 g of oleic acid-modified nano-silica, and 8 g of emulsifier fatty alcohol polyoxyethylene ether AEO-9 were added, and the mixture was sheared and dispersed to obtain a finishing liquid. The finishing liquid was sprayed onto one side of the nylon fiber membrane using a spray gun, dried at 100 ° C for 10 min, and baked at 175 ° C for 60 s to obtain a super-hydrophobic modified nylon fiber membrane.

[0067] Comparative Example 3

[0068] Add 20 g of fluorine-modified silicone oil finishing agent and 8 g of emulsifier fatty alcohol polyoxyethylene ether AEO-9 to 100 mL of distilled water, shear and disperse to obtain a finishing liquid; use a spray gun to spray the finishing liquid onto one side of the nylon fiber membrane, dry at 100°C for 10 min, and bake at 175°C for 60 s to obtain a superhydrophobic modified nylon fiber membrane.

[0069] Comparative Example 4

[0070] (1) 30 g of hydrogenated silicone oil, 1 mL of isopropanol solution containing 0.15 mg of chloroplatinic acid, and 4 mg of inhibitor p-hydroxyanisole were added to 50 mL of toluene. The temperature was raised to 125° C. under a nitrogen atmosphere, and 0.9 g of hexafluorobutyl methacrylate was added. The reaction was stirred for 4 hours, and the solution was distilled under reduced pressure, washed with methanol, and dried to obtain a fluorine-modified silicone oil finishing agent.

[0071] (2) Add 20 g of fluorine-modified silicone oil finishing agent, 1.2 g of oleic acid-modified nano-silica, and 8 g of emulsifier fatty alcohol polyoxyethylene ether AEO-9 to 100 mL of distilled water, shear and disperse, and obtain a finishing liquid; use a spray gun to spray the finishing liquid onto one side of the nylon fiber membrane, dry at 100 ° C for 10 min, and bake at 175 ° C for 60 s to obtain a superhydrophobic modified nylon fiber membrane.

[0072] The water contact angle of superhydrophobic modified nylon fiber membrane was tested according to the method of GB / T 42694-2023.

[0073] The superhydrophobic modified nylon fiber membrane was washed 20 times according to the method of GB T 8629-2017, and then the water contact angle was tested.

[0074] Table 1 Nylon fiber membrane water contact angle test

[0075]

[0076] Comparative Example 1 is a nylon fiber membrane without surface treatment and modification, with a water contact angle of 107.7° C., and does not show super hydrophobicity.

[0077] Example 3-6: A finishing liquid is prepared by compounding a fluorine-modified silicone oil finishing agent and oleic acid-modified nano-silica. After finishing and modifying the surface of a nylon fiber membrane, trifluoromethyl and biphenyl hydrophobic structures are introduced on the surface of the fiber membrane. The organic silicon film layer has strong hydrophobicity, and the oleic acid modified nano silicon dioxide is evenly dispersed in the organic silicon film layer to form a nano-micro-convex structure, which significantly improves the surface hydrophobicity of the nylon fiber membrane and its acoustic wrapping cloth, and the water contact angle reaches 139.5-151.8°. And after washing, the water contact angle remains at 138.7-150.7°, without a significant decrease. It may be that the acrylamide-based fluorine-containing monomer contains more amide bonds, which are grafted into the hydrogen-containing silicone oil, thereby introducing amide bonds in the molecular chain of the fluorine-modified silicone oil finishing agent. After finishing the nylon fiber membrane, the amide bonds of the finishing agent can form a strong chemical interaction force with the amide bonds in the nylon fiber polyamide molecular chain, so that the organic silicon film layer can be firmly attached to the surface of the nylon fiber membrane and is difficult to wash off.

[0078] The difference between Comparative Example 2 and Example 3 is that hydrogen-containing silicone oil is used as the finishing agent instead of the fluorine-modified silicone oil finishing agent. Hydrogen-containing silicone oil does not contain trifluoromethyl and biphenyl hydrophobic structures, and the hydrophobicity and water contact angle of the organic silicon film layer formed on the surface of the nylon fiber membrane after finishing are low.

[0079] In the finishing liquid of Comparative Example 3, no oleic acid-modified nano-silica was added, so that a nano-micro-convex structure could not be formed on the surface of the nylon fiber membrane, and the water contact angle was low.

[0080] Comparative Example 4 uses common hexafluorobutyl methacrylate and hydrogenated silicone oil to carry out silylation reaction to obtain a fluorine-modified silicone oil finishing agent. After finishing the surface of the nylon fiber membrane, the water contact angle is 134.2°, which is lower than that of Example 3. It may be that hexafluorobutyl methacrylate does not contain a hydrophobic biphenyl structure, and hexafluorobutyl methacrylate contains only one olefinic group, with fewer silylation reaction sites, and the grafting rate with hydrogenated silicone oil is lower. As a result, the hydrophobicity of the organic silicon film layer formed by finishing is lower than that of Example 3. And after washing, the water contact angle is 128.3°, and the decrease in the angle may be that the fluorine-modified silicone oil finishing agent of Comparative Example 4 does not contain an amide bond, and the interfacial force with the nylon fiber membrane is low, and it is not firmly attached to the surface of the nylon fiber membrane.

[0081] Example 7

[0082] The difference between this embodiment and embodiment 5 is that the amount of oleic acid-modified nano-silica used is 2.4 g.

[0083] (2) Add 20 g of fluorine-modified silicone oil finishing agent, 2.4 g of oleic acid-modified nano-silica, and 12 g of emulsifier fatty alcohol polyoxyethylene ether AEO-9 to 100 mL of distilled water, shear and disperse, and obtain a finishing liquid; use a spray gun to spray the finishing liquid onto one side of the nylon fiber membrane, dry at 90°C for 15 min, and bake at 180°C for 30 s to obtain a superhydrophobic modified nylon fiber membrane.

[0084] Example 8

[0085] The difference between this embodiment and embodiment 5 is that the amount of oleic acid-modified nano-silica used is 3.6 g.

[0086] (2) Add 20 g of fluorine-modified silicone oil finishing agent, 3.6 g of oleic acid-modified nano-silica, and 12 g of emulsifier fatty alcohol polyoxyethylene ether AEO-9 to 100 mL of distilled water, shear and disperse, and obtain a finishing liquid; use a spray gun to spray the finishing liquid onto one side of the nylon fiber membrane, dry at 90°C for 15 min, and bake at 180°C for 30 s to obtain a superhydrophobic modified nylon fiber membrane.

[0087] Example 9

[0088] The difference between this embodiment and embodiment 5 is that the amount of oleic acid-modified nano-silica used is 5 g.

[0089] (2) Add 20 g of fluorine-modified silicone oil finishing agent, 5 g of oleic acid-modified nano-silica, and 12 g of emulsifier fatty alcohol polyoxyethylene ether AEO-9 to 100 mL of distilled water, shear and disperse, and obtain a finishing liquid; use a spray gun to spray the finishing liquid onto one side of the nylon fiber membrane, dry at 90°C for 15 min, and bake at 180°C for 30 s to obtain a superhydrophobic modified nylon fiber membrane.

[0090] Table 2 Water contact angle test of nylon fiber membrane

[0091] Water contact angle (°) Example 5 151.8 Example 7 158.2 Example 8 157.3 Example 9 153.8

[0092] As the amount of oleic acid-modified nano-silica gradually increased, the water contact angle of the nylon fiber membrane reached 151.8-158.2°, showing a unique superhydrophobic property. The water contact angle showed a trend of first increasing and then decreasing. It may be that the amount of nano-silica used was too much, resulting in its poor dispersion, easy agglomeration, and failure to form a good nano-microconvex structure, which led to a decrease in the water contact angle.

[0093] The present invention also provides a method for bonding a waterproof and dustproof speaker cover cloth: a super-hydrophobic modified nylon fiber membrane is made into a speaker cover cloth that matches the size and shape of a speaker cover, and then the side of the fiber membrane that is not sprayed with a finishing liquid is hot-pressed and bonded to the speaker cover through a hot-melt adhesive film.

[0094] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a waterproof and dustproof speaker cover cloth, characterized in that: The material of the speaker cover cloth is super hydrophobic modified nylon fiber membrane; The preparation method of the super hydrophobic modified nylon fiber membrane is: (1) Add hydrogen-containing silicone oil, isopropanol solution of chloroplatinic acid, and inhibitor p-hydroxyanisole to toluene, raise the temperature to the reaction temperature under a nitrogen atmosphere, and add the structural formula acrylamide-based fluorine-containing monomer, stirring for reaction, distilling the solution under reduced pressure, washing, and drying to obtain a fluorine-modified silicone oil finishing agent; (2) adding fluorine-modified silicone oil finishing agent, oleic acid-modified nano-silica, and an emulsifier to distilled water, shearing and dispersing, and obtaining a finishing liquid; spraying the finishing liquid onto one side of a nylon fiber membrane using a spray gun, drying, and baking, and obtaining a super-hydrophobic modified nylon fiber membrane.

2. The method for preparing a waterproof and dustproof speaker cover cloth according to claim 1, characterized in that: The mass of the acrylamide-based fluorine-containing monomer in (1) is 3-15% of the mass of the hydrogen-containing silicone oil.

3. The method for preparing a waterproof and dustproof speaker cover cloth according to claim 1, characterized in that: The reaction temperature in (1) is 110-125°C and the reaction time is 4-8h.

4. The method for preparing a waterproof and dustproof speaker cover cloth according to claim 1, characterized in that: The mass of the emulsifier and oleic acid-modified nano-silica in (2) is 6-25% and 40-60% of the mass of the fluorine-modified silicone oil finishing agent, respectively.

5. The method for preparing a waterproof and dustproof speaker cover cloth according to claim 4, characterized in that: The emulsifiers include OP-10 and fatty alcohol polyoxyethylene ether AEO-9.

6. The method for preparing a waterproof and dustproof speaker cover cloth according to claim 1, characterized in that: The drying temperature in (2) is 90-100° C., the time is 10-20 min, and the baking temperature is 170-180° C., the time is 30-60 s.

7. The method for preparing a waterproof and dustproof speaker cover cloth according to claim 2, characterized in that: The preparation method of the acrylamide-based fluorine-containing monomer is: S1. Add 3-bromo-5-(trifluoromethyl)aniline and 3-amino-5-trifluoromethylphenylboronic acid pinacol ester to toluene, stir and add bistriphenylphosphine palladium dichloride and potassium carbonate, raise the temperature to 75-90° C. under nitrogen atmosphere, react for 24-36 hours, distill the solution under reduced pressure, wash, and recrystallize to obtain an aniline-based fluorine-containing monomer; S2. Add aniline-based fluorinated monomer and triethylamine to dichloromethane at 0-5°C, add acryloyl chloride dropwise after stirring, and then react at room temperature for 12-18 hours. Distill the solution under reduced pressure, wash, and recrystallize to obtain acrylamide-based fluorinated monomer.

8. The method for preparing a waterproof and dustproof speaker cover cloth according to claim 7, characterized in that: In S1, the mass of 3-amino-5-trifluoromethylphenylboronic acid pinacol ester is 125-140% of the mass of 3-bromo-5-(trifluoromethyl)aniline.

9. The method for preparing a waterproof and dustproof speaker cover cloth according to claim 7, characterized in that: In the S2, the mass of acryloyl chloride is 60-68% of the mass of the aniline-based fluorinated monomer.

10. A method for laminating a waterproof and dustproof speaker cover cloth obtained by the preparation method according to any one of claims 1 to 9, characterized in that: The bonding method is: the super-hydrophobic modified nylon fiber membrane is made into a speaker cover cloth that matches the size and shape of the speaker cover, and then the side of the fiber membrane that is not sprayed with the finishing liquid is hot-pressed and bonded to the speaker cover through a hot-melt adhesive film.

Citation Information

Patent Citations

  • Method of preparing fluorine and silicon containing hydrophobic and oil repellent fabric finishing agent

    CN101016697A

  • Super-hydrophobic transparent thin film taking hydrogen containing silicone oil cured material as matrix and preparation method thereof

    CN102140251A

  • Waterproof wear-resistant paper-plastic composite bag and preparation method thereof

    CN116587714A

  • Weather-resistant easy-to-clean fluorosilicone modified acrylic anti-doodling coating and preparation method thereof

    CN119119821A