Novel stranded PP flame-retardant net-shaped filling rope and production process thereof
By blending PP resin, flame retardant, and antioxidant, and combining spraying and vacuum impregnation technologies, an external flame retardant coating and an antioxidant layer are formed. This solves the problems of limited raw material selection and uncertain tensile strength, and improves the flame retardant performance and safety of the stranded PP flame retardant mesh filler rope.
Patent Information
- Application Number
- CN202411050602.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
AI Technical Summary
In the existing production process of polypropylene mesh filler rope, the selection of raw materials is limited and the tensile and oxidation resistance are highly uncertain, which affects the safety of use.
The process involves blending PP resin, flame retardant, defoamer, and antioxidant. An outer flame-retardant coating and two antioxidant layers are formed through spraying and vacuum impregnation. Combined with the laying of fiberglass mesh, a stranded PP flame-retardant mesh filling rope is formed.
It reduces restrictions on raw material selection, improves flame retardant performance and safety of use, and enhances the overall performance of the stranded PP flame retardant mesh filler rope.
Smart Images

Figure CN118979400A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of parallel stranded PP flame-retardant mesh filling ropes, and in particular relates to a novel parallel stranded PP flame-retardant mesh filling rope and a production process thereof. Background Art
[0002] During the cable production process, the selection of filling materials has an important impact on the overall performance of the cable. Although traditional filling materials such as filling ropes and filling strips meet the needs of cable production to a certain extent, they still have shortcomings in flame retardancy, mechanical strength and stability. Therefore, the development of new high-performance filling materials has become an important research direction in the cable industry.
[0003] As a new type of filling material, the stranded PP flame retardant mesh filling rope has been widely used in the cable industry due to its excellent flame retardant properties, high strength and good flexibility.
[0004] Chinese Patent No. 201910539946.8 discloses a production process for polypropylene mesh filling ropes, including: preparing and weighing 55-70 parts of polypropylene resin, 2-5 parts of silane coupling agent, 2-3 parts of antioxidant, 6-10 parts of polyethylene, 2-3 parts of stearic acid, 1-1.5 parts of defoaming agent and 0.8-1.5 parts of viscose; adding the prepared raw materials into a high-speed mixer for stirring; after mixing evenly, opening the high-speed mixer to discharge the materials, the evenly mixed materials need to be spread out and cooled naturally to prevent the materials from cooling and agglomerating when they are in a backlog state; after the materials are cooled, they are sent to the hopper of a twin-screw extruder through an automatic feeder, and the feeding speed is adjusted according to the material consumption in production; a twin-screw extruder is used for extrusion and film drawing, and the materials are extruded. The film is melted, mixed and plasticized in the machine, and is evenly plasticized, and is shaped into a film through a special die head; the shaped film is cooled in a water tank for stretching; the film is stretched and flattened by a first stretching machine, and the first stretching machine is equipped with a slitting blade, and the cooled film is slit into different widths according to requirements; the slit film is heated and stretched, and the stretched film is not easy to deform; the film is torn into a mesh fiber body by a mesh opening machine, and the film after the mesh is opened is not easy to bulge when the cable is filled; the film after the mesh is opened and fiberized is stretched to a winding machine through a five-roller stretching machine; the film is wound to obtain a semi-finished polypropylene mesh filling rope; the semi-finished polypropylene mesh filling rope is stranded to obtain a finished polypropylene mesh filling rope of a required diameter.
[0005] The above-mentioned polypropylene mesh filling rope production process has the following disadvantages:
[0006] 1. Due to the different properties of different silane coupling agents, antioxidants, polyethylene, stearic acid, defoamers and viscose, it is necessary to select suitable silane coupling agents, antioxidants, polyethylene, stearic acid, defoamers and viscose when blending to produce polypropylene mesh filling ropes to ensure production quality, which limits the choice of raw materials and increases the difficulty of producing polypropylene mesh filling ropes;
[0007] 2. The polypropylene mesh filling rope is made by blending polypropylene resin, silane coupling agent, antioxidant, polyethylene, stearic acid, defoaming agent and viscose, cooling, extruding, cooling, slitting, stretching, opening, winding and stranding. The tensile and antioxidant strength of the polypropylene mesh filling rope is determined by the uniformity of the raw materials in the blending stage, which is uncertain, reducing the safety of the use of the polypropylene mesh filling rope.
[0008] In view of this, a new type of parallel stranded PP flame retardant mesh filling rope and its production process are designed to solve the above problems. Summary of the invention
[0009] To solve the problems raised in the above background technology, the present invention provides a novel stranded PP flame retardant mesh filling rope and its production process, which has the characteristics of reducing the restrictions on raw material selection to a certain extent and improving the safety of the stranded PP flame retardant mesh filling rope.
[0010] Another object of the present invention is to provide a production process for a novel stranded PP flame-retardant mesh filling rope.
[0011] To achieve the above object, the present invention provides the following technical solution: a novel stranded PP flame-retardant mesh filling rope, comprising the following raw materials:
[0012] PP resin, flame retardant, defoamer and antioxidant.
[0013] Furthermore, the flame retardant comprises the following raw materials: ammonium polyphosphate, pentaerythritol, melamine, silicone powder, dispersant and viscose.
[0014] Furthermore, the defoaming agent includes the following raw materials: silicone oil defoaming agent.
[0015] Furthermore, the antioxidant comprises the following raw materials: antioxidant 1010 and viscose.
[0016] The production process of the novel stranded PP flame-retardant mesh filling rope comprises the following steps:
[0017] S1: Prepare the following raw materials, including PP resin, flame retardant, defoamer and antioxidant;
[0018] S2: Add PP resin, flame retardant and defoamer into a high-speed mixer according to the proportion and mix them evenly;
[0019] S3: The uniformly mixed materials are fed into a twin-screw extruder, melted and extruded under high temperature and high pressure;
[0020] S4: sending the extruded material into a water tank for cooling;
[0021] S5: The cooled material is sent to the stretching and slitting machine, where it is stretched and slit into materials of specific diameter and shape according to requirements;
[0022] S6: Send the stretched and cut materials into the spraying machine, spray the flame retardant evenly on the surface of the materials, and evacuate the materials to allow the flame retardant to penetrate into the surface and inside of the materials;
[0023] S7: sending the vacuum impregnated material into an air cooling machine for air drying and forming an outer flame retardant coating;
[0024] S8: sending the air-dried and formed material into a glass fiber mesh laying machine, and evenly laying the glass fiber mesh on the outer flame retardant coating surface of the material;
[0025] S9: feeding the material with the glass fiber mesh into the spraying machine, spraying the antioxidant evenly on the surface of the glass fiber mesh, and evacuating the vacuum to allow the antioxidant to penetrate into the inside of the glass fiber mesh and the surface and inside of the outer flame retardant coating;
[0026] S10: sending the vacuum impregnated material into an air cooling machine for air drying and forming the first outer anti-oxidation coating;
[0027] S11: sending the air-dried and formed material into a glass fiber mesh laying machine, and evenly laying the glass fiber mesh on the surface of the first outer anti-oxidation coating of the material;
[0028] S12: feeding the material with the glass fiber mesh into a spraying machine, spraying the antioxidant evenly on the surface of the glass fiber mesh, and evacuating the vacuum to allow the antioxidant to penetrate into the inside of the glass fiber mesh and the surface and inside of the first outer anti-oxidation coating;
[0029] S13: sending the vacuum impregnated material into an air cooling machine for air drying and forming a second outer anti-oxidation coating, i.e., a semi-finished PP flame-retardant mesh filling rope;
[0030] S14: sending a plurality of single-strand PP flame-retardant mesh filling rope semi-finished products into a twisting machine, combining the plurality of single-strand PP flame-retardant mesh filling ropes and then twisting them, that is, a new type of twisted PP flame-retardant mesh filling rope.
[0031] Furthermore, in step S2, the input ratio of PP resin, flame retardant and defoaming agent is 78-80%: 16-19%: 1-6%.
[0032] Furthermore, in step S11, the laid glass fiber mesh is laid alternately with the glass fiber mesh in the first outer anti-oxidation coating layer, that is, the mesh openings of the laid glass fiber mesh correspond to the mesh wires of the glass fiber mesh in the first outer anti-oxidation coating layer.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] 1. The present invention firstly mixes PP resin, flame retardant and defoamer to form a material, then forms an outer flame retardant coating by spraying, vacuum impregnation and air drying, then forms two outer anti-oxidation layers by spraying, laying glass fiber mesh, vacuum impregnation and air drying, and finally forms a parallel strand PP flame retardant mesh filling rope by merging and twisting. Compared with the prior art, the production of the parallel strand PP flame retardant mesh filling rope has less raw materials in each process, which reduces the limitation of raw material selection to a certain extent.
[0035] 2. The present invention firstly prepares a material by blending PP resin, flame retardant and defoaming agent, and then prepares an outer flame retardant coating by spraying, vacuum impregnation and air drying, and then prepares two outer anti-oxidation layers by spraying, laying glass fiber mesh, vacuum impregnation and air drying, and finally forms a parallel stranded PP flame retardant mesh filling rope by merging and twisting. Compared with the prior art, the flame retardant performance of the parallel stranded PP flame retardant mesh filling rope depends not only on the uniformity of the internally blended flame retardant, but also on the flame retardant uniformly impregnated externally, thereby improving the flame retardancy of the parallel stranded PP flame retardant mesh filling rope, that is, improving the use safety of the parallel stranded PP flame retardant mesh filling rope. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 The present invention is a flow chart of the production process of the novel stranded PP flame-retardant mesh filling rope. DETAILED DESCRIPTION
[0037] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] A new type of stranded PP flame-retardant mesh filling rope, including the following raw materials:
[0039] PP resin, flame retardant, defoamer and antioxidant.
[0040] In this embodiment, the input ratio of PP resin, flame retardant and defoamer in the blending stage is 78-80%: 16-19%: 1-6%, the input ratio of flame retardant in the spraying stage is 1.5-2%, and the input ratio of antioxidant in the spraying stage is 0.2-0.4%;
[0041] Preferably, the input ratio of PP resin, flame retardant and defoaming agent in the blending stage is 78%:19%:3%, the input ratio of flame retardant in the spraying stage is 1.6%, and the input ratio of antioxidant in the spraying stage is 0.4%.
[0042] Specifically, the flame retardant includes the following raw materials: ammonium polyphosphate, pentaerythritol, melamine, silicone powder, dispersant and viscose.
[0043] In this embodiment, the input ratio of ammonium polyphosphate, pentaerythritol, melamine, silicone powder, dispersant and viscose is 20%-50%: 5%-15%: 10%-25%: 0.1%-5%: 0.5%-5%: 5%-10%.
[0044] Preferably, the input ratio of ammonium polyphosphate, pentaerythritol, melamine, silicone powder, dispersant and viscose is 47%:13%:25%:5%:4.5%:5.5%.
[0045] Specifically, the defoaming agent includes the following raw materials: silicone oil defoaming agent.
[0046] Specifically, the antioxidant includes the following raw materials: antioxidant 1010 and viscose.
[0047] In this embodiment, the input ratio of antioxidant 1010 and viscose is 80-85%:15-20%;
[0048] Preferably, the input ratio of antioxidant 1010, dispersant and viscose is 82%:18%.
[0049] A production process of a novel stranded PP flame-retardant mesh filling rope comprises the following steps:
[0050] S1: Prepare the following raw materials, including PP resin, flame retardant, defoamer and antioxidant;
[0051] S2: Add PP resin, flame retardant and defoamer into a high-speed mixer according to the proportion and mix them evenly;
[0052] In this embodiment, the mixing temperature of the high-speed mixer is 100-120°C, the mixing speed is 3000-5000r / min, and the mixing time is 20-30min;
[0053] Preferably, the mixing temperature of the high-speed mixer is 120°C, the mixing speed is 5000r / min, and the mixing time is 20min;
[0054] S3: The uniformly mixed materials are fed into a twin-screw extruder, melted and extruded under high temperature and high pressure;
[0055] In this embodiment, the twin-screw extruder is divided into nine temperature zones, and the temperatures of the nine zones are: zone 1 150-160°C, zones 2 to 4 160-170°C, zones 5 to 7 165-180°C, and zones 8 to 9 160-170°C; the die head is divided into three temperature zones, and the temperatures of the three zones are: zone 1 160-170°C, zone 2 165-175°C, and zone 3 150-160°C;
[0056] Preferably, the temperatures of the nine zones are: 150°C for zone 1, 160°C for zones 2 to 4, 180°C for zones 5 to 7, and 170°C for zones 8 to 9; the die head is divided into three zones, and the temperatures of the three zones are: 160°C for zone 1, 175°C for zone 2, and 160°C for zone 3;
[0057] S4: sending the extruded material into a water tank for cooling;
[0058] In this embodiment, the temperature of the water tank is 30-50°C;
[0059] Preferably the temperature of the water tank is 40°C;
[0060] S5: The cooled material is sent to the stretching and slitting machine, where it is stretched and slit into materials of specific diameter and shape according to requirements;
[0061] S6: Send the stretched and cut materials into the spraying machine, spray the flame retardant evenly on the surface of the materials, and evacuate the materials to allow the flame retardant to penetrate into the surface and inside of the materials;
[0062] In this embodiment, the spraying pressure of the sprayer is 0.5-0.6MPa, and the spraying speed is 0.4-0.6m / s;
[0063] Preferably, the spraying pressure of the sprayer is 0.6 MPa and the spraying speed is 0.5 m / s;
[0064] S7: sending the vacuum impregnated material into an air cooling machine for air drying and forming an outer flame retardant coating;
[0065] In this embodiment, the cooling rate of the air cooler is 50-60°C / min;
[0066] Preferably, the cooling rate of the air cooler is 60°C / min;
[0067] S8: sending the air-dried and formed material into a glass fiber mesh laying machine, and evenly laying the glass fiber mesh on the outer flame retardant coating surface of the material;
[0068] S9: feeding the material with the glass fiber mesh into the spraying machine, spraying the antioxidant evenly on the surface of the glass fiber mesh, and evacuating the vacuum to allow the antioxidant to penetrate into the inside of the glass fiber mesh and the surface and inside of the outer flame retardant coating;
[0069] In this embodiment, the spraying pressure of the sprayer is 0.5-0.6MPa, and the spraying speed is 0.4-0.6m / s;
[0070] Preferably, the spraying pressure of the sprayer is 0.6 MPa and the spraying speed is 0.5 m / s;
[0071] S10: sending the vacuum impregnated material into an air cooling machine for air drying and forming the first outer anti-oxidation coating;
[0072] In this embodiment, the cooling rate of the air cooler is 50-60°C / min;
[0073] Preferably, the cooling rate of the air cooler is 50°C / min;
[0074] S11: sending the air-dried and formed material into a glass fiber mesh laying machine, and evenly laying the glass fiber mesh on the surface of the first outer anti-oxidation coating of the material;
[0075] S12: feeding the material with the glass fiber mesh into a spraying machine, spraying the antioxidant evenly on the surface of the glass fiber mesh, and evacuating the vacuum to allow the antioxidant to penetrate into the inside of the glass fiber mesh and the surface and inside of the first outer anti-oxidation coating;
[0076] In this embodiment, the spraying pressure of the sprayer is 0.5-0.6MPa, and the spraying speed is 0.4-0.6m / s;
[0077] Preferably, the spraying pressure of the sprayer is 0.6 MPa and the spraying speed is 0.5 m / s;
[0078] S13: sending the vacuum impregnated material into an air cooling machine for air drying and forming a second outer anti-oxidation coating, i.e., a semi-finished PP flame-retardant mesh filling rope;
[0079] In this embodiment, the cooling rate of the air cooler is 50-60°C / min;
[0080] Preferably, the cooling rate of the air cooler is 50°C / min;
[0081] S14: sending a plurality of single-strand PP flame-retardant mesh filling rope semi-finished products into a twisting machine, combining the plurality of single-strand PP flame-retardant mesh filling ropes and then twisting them, that is, a new type of twisted PP flame-retardant mesh filling rope.
[0082] Specifically, in step S11, the laid glass fiber mesh is laid alternately with the glass fiber mesh in the first outer anti-oxidation coating layer, that is, the mesh openings of the laid glass fiber mesh correspond to the mesh wires of the glass fiber mesh in the first outer anti-oxidation coating layer.
[0083] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A new type of parallel stranded PP flame retardant mesh filling rope, characterized in that: Including the following ingredients: PP resin, flame retardant, defoamer and antioxidant.
2. The novel parallel strand PP flame retardant mesh filling rope according to claim 1 is characterized in that: The flame retardant comprises the following raw materials: ammonium polyphosphate, pentaerythritol, melamine, silicone powder, dispersant and viscose.
3. The novel parallel strand PP flame retardant mesh filling rope according to claim 1 is characterized in that: The defoaming agent comprises the following raw materials: silicone oil defoaming agent.
4. The novel parallel strand PP flame retardant mesh filling rope according to claim 1 is characterized in that: The antioxidant comprises the following raw materials: antioxidant 1010 and viscose.
5. The production process of a novel parallel stranded PP flame retardant mesh filling rope according to claims 1-4, characterized in that: The following steps are involved: S1: Prepare the following raw materials, including PP resin, flame retardant, defoamer and antioxidant; S2: Add PP resin, flame retardant and defoamer into a high-speed mixer according to the proportion and mix them evenly; S3: The uniformly mixed materials are fed into a twin-screw extruder, melted and extruded under high temperature and high pressure; S4: sending the extruded material into a water tank for cooling; S5: The cooled material is sent to the stretching and slitting machine, where it is stretched and slit into materials of specific diameter and shape according to requirements; S6: Send the stretched and cut materials into the spraying machine, spray the flame retardant evenly on the surface of the materials, and evacuate the materials to allow the flame retardant to penetrate into the surface and inside of the materials; S7: sending the vacuum impregnated material into an air cooling machine for air drying and forming an outer flame retardant coating; S8: sending the air-dried and formed material into a glass fiber mesh laying machine, and evenly laying the glass fiber mesh on the outer flame retardant coating surface of the material; S9: feeding the material with the glass fiber mesh into the spraying machine, spraying the antioxidant evenly on the surface of the glass fiber mesh, and evacuating the vacuum to allow the antioxidant to penetrate into the inside of the glass fiber mesh and the surface and inside of the outer flame retardant coating; S10: sending the vacuum impregnated material into an air cooling machine for air drying and forming the first outer anti-oxidation coating; S11: sending the air-dried and formed material into a glass fiber mesh laying machine, and evenly laying the glass fiber mesh on the surface of the first outer anti-oxidation coating of the material; S12: feeding the material with the glass fiber mesh into a spraying machine, spraying the antioxidant evenly on the surface of the glass fiber mesh, and evacuating the vacuum to allow the antioxidant to penetrate into the inside of the glass fiber mesh and the surface and inside of the first outer anti-oxidation coating; S13: sending the vacuum impregnated material into an air cooling machine for air drying and forming a second outer anti-oxidation coating, i.e., a semi-finished PP flame-retardant mesh filling rope; S14: sending a plurality of single-strand PP flame-retardant mesh filling rope semi-finished products into a twisting machine, combining the plurality of single-strand PP flame-retardant mesh filling ropes and then twisting them, that is, a new type of twisted PP flame-retardant mesh filling rope.
6. The production process of a novel parallel stranded PP flame retardant mesh filling rope according to claim 5 is characterized by: In the step S2, the input ratio of PP resin, flame retardant and defoaming agent is 78-80%: 16-19%: 1-6%.
7. The production process of a novel parallel stranded PP flame retardant mesh filling rope according to claim 5 is characterized by: In the step S11, the laid glass fiber mesh is laid alternately with the glass fiber mesh in the first outer anti-oxidation coating layer, that is, the mesh openings of the laid glass fiber mesh correspond to the mesh wires of the glass fiber mesh in the first outer anti-oxidation coating layer.
Citation Information
Patent Citations
Production process of polypropylene reticular filling rope
CN112111098A
High-flame-retardant fire-resistant cable filling rope and preparation method thereof
CN113445340A
Composite environment-friendly high-flame-retardant filling rope for flame-retardant fire-resistant cable and preparation method thereof
CN114318848A
Production process of high-tensile polypropylene net-shaped filling rope
CN114474644A
High-toughness filling rope