Titan rock plate
Through the design of Titan rock slabs, the composite integrated molding of modified aluminosilicate gelling material and thermal insulation cotton and polyurethane elastic adhesive bonding are solved, and the problems of deformation and glue falling off of composite aluminum plates under high and low temperature cycles are used. It achieves high stability and durability of the board, and meets the waterproof, fireproof and thermal insulation performance that meets construction needs.
Patent Information
- Application Number
- CN202411064994.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-19
AI Technical Summary
Integrated composite aluminum plates are prone to deformation and drumming and joint glue falling off under high and low temperature cycles, which affects their flatness and durability.
The design of Titanite slabs is adopted, including calcium silicate slab layer, composite core layer, A2-level fire-resistant core material and silk aluminum leather. It is formed by the composite integrated molding of modified aluminosilicate gelling material and thermal insulation cotton, combined with polyurethane elasticity The structural design of adhesive bonding, anchor bolts and stainless steel fasteners enhances the flatness and durability of the sheet.
It significantly improves the stability and durability of the board under high and low temperature cycles, reduces deformation and joint glue falling off, ensures the long-term stability and safety of the building exterior walls, and also has excellent waterproof, fireproof and thermal insulation performance.
Smart Images

Figure CN118979587A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of building panels, and in particular to Titanite panels. Background Art
[0002] In recent years, with the rapid development of the construction industry and the country's active call for energy conservation and environmental protection, in order to meet people's growing demand for building exterior walls, integrated composite aluminum panels combining aluminum and other functional materials have been widely used in new doors, windows and curtain wall building materials.
[0003] This integrated composite aluminum profile is gradually becoming a popular choice in the construction industry due to its unique advantages. By combining with other functional materials, the strength of this profile has been further improved, ensuring the long-term stability of the building's exterior wall. However, due to the characteristics of aluminum itself and the combination with other materials, it is easy to cause deformation and bulging after high and low temperature cycles, and the glue that maintains the connection between them will also fall off, which greatly reduces the flatness of the integrated composite aluminum profile. To solve this problem, a special Titan rock plate is provided. Summary of the invention
[0004] In order to solve the problems of deformation, bulging and falling off of connecting glue of integrated composite aluminum plates under high and low temperature cycles in related technologies, the present application provides a Titan stone plate, which aims to enhance the flatness and durability of the plate by improving the material composition and structural design, while ensuring its fireproof, waterproof and thermal insulation properties, so as to adapt to different climatic conditions and construction requirements and ensure the long-term stability and safety of the building exterior wall.
[0005] The Titanite slab provided in this application adopts the following technical solutions: Titanite board, including calcium silicate board layer, composite core layer, calcium silicate board layer, A2 grade fireproof core material and silk aluminum skin layer arranged in sequence; The composite core layer is formed by composite integration of modified aluminum silicate gelling material and thermal insulation cotton; The raw materials for preparing the modified aluminosilicate gelling material include the following components in weight fractions: 60-80 parts of aluminosilicate, 3-6 parts of nano whisker cellulose, and 5-10 parts of 2-methoxyethyl acrylate, and are prepared by the following preparation method: S1, adding aluminosilicate, nano whisker cellulose and 2-methoxyethyl acrylate to a methanol aqueous solution, slowly adding citric acid dropwise while stirring, and mixing well to obtain a mixed solution A; S2, adjusting the pH and temperature of the mixed solution A obtained in S1, and cooling after continuous stirring to obtain a viscous mixture B; S3, drying the viscous mixture B obtained in S2, and grinding it to obtain a modified aluminosilicate gelling material with a certain particle size distribution.
[0006] By adopting the above technical solution: a high-performance Titanite board material can be obtained, which has excellent flatness and durability, good resistance to high and low temperature cycles, good environmental performance, meets the requirements of sustainable development, and is excellent in waterproof and fireproof performance.
[0007] The reasons may be: We designed a composite core layer that includes modified aluminosilicate gelling materials and thermal insulation cotton, and these materials are tightly combined together through composite integrated molding. This design greatly enhances the flatness and durability of the board. In particular, the performance of the modified aluminosilicate gelling materials has been significantly improved after a specific preparation process optimization. The gel structure formed by the modified aluminosilicate gelling materials during the preparation process has excellent colloidal dispersibility, suspension, thickening and thixotropy, which enables the board to maintain a high degree of flatness and durability after molding. Other materials may not be able to provide such excellent physical properties, and as the main component of the composite core layer, it can form good compatibility and bonding with other layers (such as calcium silicate board layer, A2 grade fireproof core material and silk aluminum skin layer).
[0008] Preferably, the wire-aluminum skin layer is formed by bonding wire-aluminum skins.
[0009] Preferably, the A2-grade fireproof core material is formed by pressing a calcium silicate board and a fireproof composite plastic into one piece.
[0010] By adopting the above technical solution: the calcium silicate board has higher strength and stability, and is not easily deformed due to temperature changes. The addition of fire-resistant composite plastic can further increase the rigidity and flatness of the board, reduce the deformation caused by temperature fluctuations, and the use of A2-grade fire-resistant core material that is pressed and molded in one piece can ensure that there are no gaps or voids between the materials, further improving the thermal insulation and flame retardant properties.
[0011] Preferably, the calcium silicate board layer and the composite core layer, the composite core layer and the A2-grade fireproof core material, and the A2-grade fireproof core material and the wire aluminum skin layer are bonded by polyurethane elastic adhesive, and the polyurethane elastic adhesive forms a bonding layer after curing.
[0012] By adopting the above technical solution, a firm and stable connection between the layers of the plate is achieved, and at the same time, the deformation of the aluminum plate caused by temperature changes can be alleviated to a certain extent, further enhancing the flatness and durability of the plate.
[0013] Preferably, an anchor bolt is provided on the composite core layer, the head of the anchor bolt is pre-buried in the composite core layer, and the screw rod of the anchor bolt passes through the composite core layer and the calcium silicate board layer in sequence.
[0014] By adopting the above technical solution: a firm connection between the composite core layer and the calcium silicate board layer can be ensured, and the separation or displacement of the board layer under high and low temperature cycles or external forces can be effectively prevented. The head of the anchor bolt is embedded in the composite core layer, which increases the strength and stability of the connection point, and the screw passes through the composite core layer and the calcium silicate board layer to form a reliable fixed structure.
[0015] Preferably, stainless steel fasteners are provided on the sides of the wire aluminum skin layer for connection and fixation with the wall.
[0016] By adopting the above technical solution: a stable connection with the wall is achieved, and its wind pressure resistance, earthquake resistance and other performances are improved, further enhancing the overall stability and safety of the Titan rock slab.
[0017] The method for preparing a Titanite plate comprises the following steps: A1. Preparation of calcium silicate board layer: pretreating the calcium silicate board to obtain the calcium silicate board layer; A2. Preparation of a composite core layer: Lay the thermal insulation cotton in a predetermined mold, perform pre-pressing first, then add the modified aluminum silicate gelling material to a 0.6%wt% aqueous solution of methacryloxysilane and mix evenly to obtain a modified aluminum silicate gelling liquid, then fill the modified aluminum silicate gelling liquid into the mold, apply appropriate pressure, demould after curing, perform subsequent processing operations, and obtain a composite core layer; Preparation of A2-grade fireproof core material (3): molten glass fiber is mixed with aluminum hydroxide and phosphate and then filled into a mold, and pressed and molded at the same time, and then post-processed after cooling and molding; A4. Assembly: Apply polyurethane elastic glue on the surface of the calcium silicate board layer, A2-grade fireproof core material and composite core layer, and then adhere the silk aluminum skin to the A2-grade fireproof core material to form a silk aluminum skin layer. Then, open connecting holes on the composite core layer and install stainless steel fasteners on the side of the A2-grade fireproof core material, insert anchor bolts into the connecting holes, bond the calcium silicate board layer, silk aluminum skin layer, A2-grade fireproof core material and composite core layer together, apply appropriate pressure, and obtain the Titanite slab after solidification.
[0018] Preferably, the curing temperature in A2 is 260-290°C.
[0019] Preferably, the post-processing operation in A3 includes one or more of surface cleaning, activation treatment, and cutting.
[0020] By adopting the above technical solution: this preparation method has the advantages of simple operation, high production efficiency, stable product quality, etc., and can meet the needs of different construction projects.
[0021] In summary, the present application includes at least one of the following beneficial technical effects: 1. The Titanite board made by the present application using calcium silicate board, thermal insulation cotton and modified aluminum silicate cementitious materials can maintain stability under high and low temperature cycles, significantly reducing the problems of deformation, bulging and connection glue falling off caused by temperature changes. This temperature resistance ensures the long-term reliability of the structure under different climatic conditions; 2. The gel structure formed by the modified aluminosilicate gelling material in the present application during the preparation process has excellent colloidal dispersibility, suspension, thickening and thixotropy, which enables the board to maintain high flatness and durability after molding; 3. The design of the Titan stone slab takes into account the performance of the material, the stability of the structure and the ease of assembly. Through carefully designed preparation processes such as pre-pressing, curing and appropriate pressure application, the high quality and long-term stability of the structure are ensured. In addition, the use of high-performance cementitious materials and adhesives, such as polyurethane elastic glue, further enhances the connection strength and durability between the structures. This optimized structural design and preparation process enables the Titan stone slab to meet different construction needs and provide long-lasting and stable performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a schematic diagram of the overall structure of the Titanite slab in Example 1 of the present application; Figure 2 It is a schematic diagram of the partial cross-sectional structure of the Titanite slab in Example 1 of the present application.
[0023] Figure numerals: 1, calcium silicate board layer; 2, composite core layer; 21, anchor bolt; 3, A2 grade fireproof core material; 31, stainless steel fastener; 4, bonding layer; 5, wire aluminum skin layer. DETAILED DESCRIPTION
[0024] The following is combined with the embodiments and the attached Figure 1-2 To further explain the present application in detail, the raw materials used in the present application are all common commercially available materials except for the following special instructions.
[0025] Preparation Example Preparation Example 1 A modified aluminosilicate gelling material, whose components and relative amounts are shown in the following table, is prepared by the following preparation method: S1, adding aluminosilicate, nano whisker cellulose, and 2-methoxyethyl acrylate into a reaction kettle, adding 80wt% methanol aqueous solution into the reaction kettle until all the raw materials are immersed, slowly dropping 1% of citric acid accounting for the total weight of the mixed solution while stirring, the dropping rate is 500g / min, and mixing evenly to obtain a mixed solution A; S2, adjusting the pH of the mixed solution A obtained in S1 to 3.6 and heating it to 156°C, stirring it for 4 hours and then cooling it to 35°C to obtain a viscous mixture B; S3. Put the viscous mixture B obtained in S2 into a drying oven, dry it at 60°C to constant weight, and then put it into a ball mill for grinding. After grinding at a speed of 3500 rpm, a modified aluminosilicate gelling material with an average particle size of 10 μm is obtained.
[0026] Table: Components and dosage in Preparation Example 1 (kg) Preparation Example 2-4 A modified aluminosilicate gelling material, which is different from Preparation Example 1 in that the amounts of the components are different, as shown in the following table: Table: Components and dosages in Preparation Examples 2-4 (kg) Preparation Example 5-8 A modified aluminosilicate gelling material, which is different from Preparation Example 1 in that the specific process conditions in the preparation steps are different, and the specific conditions are referred to the following table: Table: Comparison table of specific process conditions of preparation steps in Preparation Examples 5-8 The performance test refers to GB / T 35169-2017 "Weather Resistance Test Method for External Insulation System of Building Exterior Walls", selects the Titanite slabs prepared in the embodiments and comparative examples, and then conducts a hot and cold cycle test on them. The test is carried out for 30 rounds in the temperature range of -10°C to 60°C, and the flatness of the aluminum plate of the sample and whether there is glue shedding are observed. The average value of the test results is taken and graded and evaluated as A, B, C, D, and E. According to GB 8624-2012 “Classification of Combustion Performance of Building Materials and Products”, the Titanite panels prepared in the examples and comparative examples were selected and then flame retardancy tests were performed respectively. Example
[0027] Example 1 A Titanite slab, see Figure 1-2It includes a calcium silicate board layer 1, a composite core layer 2, a calcium silicate board layer 1, an A2-grade fireproof core material 3 and a silk aluminum skin layer 5 which are arranged in sequence, wherein the calcium silicate board layer 1 is installed on the wall, the composite core layer 2, the A2-grade fireproof core material 3, and the silk aluminum skin layer 5 are bonded to the calcium silicate board layer 1 by polyurethane elastic glue, an anchor bolt 21 is installed on the composite core layer 2, the head of the anchor bolt 21 is pre-embedded in the composite core layer 2, and the screw rod part passes through the composite core layer 2 and the calcium silicate board layer 1 in sequence, and in addition, a stainless steel fastener 32 is installed on the side of the A2-grade fireproof core material 3 to further strengthen the connection strength with the wall.
[0028] The Titanite plate is prepared by the following preparation method: A1. Preparation of calcium silicate board layer 1: The surface of the calcium silicate board is polished and cleaned, and then cut into a size of 60 mm*50 mm*5 mm to obtain the calcium silicate board layer 1; A2. Preparation of composite core layer 2: Cut the thermal insulation cotton into a size of 60 mm*50 mm*5 mm, select six pieces and stack them in a predetermined mold, pre-press them at 0.2 MPa, then add the modified aluminum silicate gelling material prepared in Preparation Example 1 to a 0.6% aqueous solution of methacryloyloxysilane and mix them evenly to obtain a modified aluminum silicate gelling liquid, then fill the modified aluminum silicate gelling liquid into the mold, apply a pressure of 0.18 MPa to it, and cure it at 286°C for 2 hours. After curing, demould, grind and cut to obtain a 30 mm composite core layer 2; Preparation of A3 and A2 grade fireproof core material 3: glass fiber, aluminum hydroxide and phosphate in a mass ratio of 1:0.3:0.005 are mixed and melted at high temperature and filled into a 60mm*50mm*3mm special mold, ensuring that it is filled to the top of the mold. After filling, a pressing device is used to apply a pressure of 0.25MPa to the mold, and after cooling and forming, it is cut and its surface is cleaned to obtain a 3mmA2 grade fireproof core material; A4. Assembly: Open a connecting hole on the composite core layer 2 and install a stainless steel fastener 32 on the side of the A2-grade fireproof core material 3, insert the anchor bolt 21 into the connecting hole, and then apply polyurethane elastic glue on the surface of the calcium silicate board layer 1, the A2-grade fireproof core material 3, the silk aluminum skin layer 5 and the composite core layer 2 respectively, bond the calcium silicate board layer 1, the silk aluminum skin layer 5, the A2-grade fireproof core material 3, and the composite core layer 2 together, apply a pressure of 0.09 MPa to them, and cure them at 90°C for 90 minutes. After the curing is completed, a bonding layer 4 is formed to obtain the Titan rock plate, wherein the bonding layer thickness is 1 mm, and the thickness of the silk aluminum skin layer 5 is 0.38 mm.
[0029] The Titanite slab prepared in Example 1 was sampled and its performance was tested according to the above-mentioned test standard. The test results are shown in the following table.
[0030] Table: Example 1 Performance Test Results It can be seen from the above table that the Titanite plate sample prepared in Example 1 still maintains excellent flatness under high and low temperature cycles, has no degumming phenomenon, and its flame retardant performance reaches Class A.
[0031] Analyze the possible reasons, which may be: 1. Material Combination The calcium silicate board layer 1 is composed of calcium silicate boards, which provide structural strength and excellent thermal insulation performance and stability. As an inorganic material, calcium silicate boards have good thermal stability and can resist deformation caused by temperature changes. The composite core layer 2 is reinforced with thermal insulation cotton and combined with modified aluminum silicate gelling materials to obtain a composite core layer 2 with stable structure and high temperature resistance; Since the aluminosilicate material itself has high thermal stability and low thermal conductivity, its ability to resist high and low temperature cycles can be significantly enhanced by adding nano-whisker cellulose and 2-methoxyethyl acrylate for modification. This enhancement is mainly attributed to the improved dispersibility of nano-whisker cellulose, enhanced interface bonding, and improved chemical stability and flexibility of 2-methoxyethyl acrylate. At the same time, the integrated composite with thermal insulation cotton further improves the performance stability of the composite board. This performance is crucial for building exterior wall materials because it needs to withstand temperature changes under different climatic conditions without deformation or bulging. In addition, the gel structure formed by the modified aluminosilicate gelling material during the preparation process has excellent colloidal dispersibility, suspension, thickening and thixotropy, which enables the board to maintain high flatness and durability after molding. Other materials may not be able to provide such excellent physical properties.
[0032] 2. Comprehensive effect of process and structural design The composite core layer 2 has been composited to enhance the material stability and durability, and the anchor bolts 21 are pre-buried in the composite core layer 2. The screw portion passes through the calcium silicate board layer 1 to enhance the interlayer connection strength, and the stainless steel fasteners 32 strengthen the connection between the Titanite board and the wall to improve the overall stability. At the same time, polyurethane elastic glue is used as a high-quality adhesive to ensure that the layers are tightly connected, and its elasticity can alleviate the deformation stress caused by temperature changes.
[0033] Embodiment 2-4 A Titanite slab is different from Example 1 in that the source of the modified aluminosilicate cementitious material used in the preparation of the composite core layer in step A2 is different, and the specific usage is shown in the following table: Table: Comparison table of usage of modified aluminosilicate gelling materials in Examples 2-4 Group Modified aluminosilicate cementitious materials Example 2 Prepared from Preparation Example 2 Example 3 Prepared from Preparation Example 3 Example 4 Prepared by Preparation Example 4 The Titanite slabs prepared in Examples 2-4 were sampled and performance tested according to the above test standards. The test results are shown in the following table.
[0034] Table: Performance test results of Examples 2-4 It can be seen from the above table that the Titanite board samples prepared by Examples 2-4 all maintain excellent flame retardancy, and as the content of aluminosilicate increases, the shrinkage of the modified aluminosilicate cementitious material during the curing process may be enhanced, causing the composite core layer 2 to shrink to a certain extent, thereby weakening the bonding force between the composite core layer 2 and the calcium silicate board layer 1 and the A2-grade fireproof core material 3, resulting in a small amount of debonding; When the content of nano-whisker cellulose is further increased, the flatness decreases by one level. This may be because the dispersion uniformity of nano-whisker cellulose in the modified aluminosilicate gelling material deteriorates. When the dispersion is uneven, the material will have uneven stress distribution during the curing process, which in turn affects the flatness.
[0035] Embodiment 5-8 A Titanite slab is different from Example 1 in that the source of the modified aluminosilicate cementitious material used in the preparation of the composite core layer in step A2 is different, and the specific usage is shown in the following table: Table: Comparison table of usage of modified aluminosilicate gelling materials in Examples 5-8 Group Modified aluminosilicate cementitious materials Example 5 Prepared from Preparation Example 5 Example 6 Prepared from Preparation Example 6 Example 7 Prepared from Preparation Example 7 Example 8 Prepared from Preparation Example 8 The Titanite slabs prepared in Examples 5-8 were selected and their performance was tested according to the above-mentioned test standards. The test results are shown in the following table.
[0036] Table: Performance test results of Examples 5-8 It can be seen from the above table that the flatness of the Titanite slabs prepared from Examples 5-8 decreased to varying degrees, and a large amount of degumming occurred in Examples 5 and 6, and a small amount of degumming occurred in Example 8. As for the flame retardant level, Examples 6 and 7 still maintained a relatively high flame retardant level, while the flame retardant level of Examples 5 and 6 decreased.
[0037] The pH values of Examples 1 and 6 are both 3.6, while the pH value of Example 5 is 9.0. Changes in pH may significantly affect the surface charge of aluminosilicate and its interaction with additives such as nano whisker cellulose and 2-methoxyethyl acrylate. Too high or too low pH may lead to instability or coagulation between particles, thereby affecting the flatness and degumming performance of the material. The pH value may also affect the flame retardant properties of the material. In some cases, a specific pH value may help to form a more stable flame retardant structure or promote the uniform dispersion of flame retardant additives. The heating temperatures of Examples 1 and 5 are both 156° C., while the heating temperature of Example 6 is 80° C. Changes in temperature may affect the chemical reaction rate of the material, the agglomeration or dispersion of particles, and the degree of curing of the material. High temperatures may help accelerate the reaction and form a more stable structure, while low temperatures may lead to incomplete reactions or insufficient curing of the material. The effect of temperature on flame retardant properties may be related to the thermal stability of the material and the activation temperature of the flame retardant additive. The temperatures in the drying oven of Example 1 and Example 7 are 60°C and 100°C, respectively. Although changes in the drying temperature may affect the drying speed and final moisture content of the material, its effect on the flame retardant properties may not be decisive unless the moisture content significantly affects the thermal stability of the material. Example 8 was not dried to constant weight, which resulted in a higher moisture content in the material, thereby affecting its flatness and degumming performance. Too high a moisture content may reduce the cohesion of the material and its adhesion to the substrate, resulting in degumming.
[0038] Example 9 A Titan rock board, which is different from Example 1 in that, in the preparation of the composite core layer in step A2, the thermal insulation cotton is cut into a specification of 60mm*50mm*5mm, ten strips are selected and stacked and laid flat in a predetermined mold, and pre-pressed at 0.2MPa, and then the modified aluminum silicate gelling material prepared in Preparation Example 1 is added to a 0.6% aqueous solution of methacryloxysilane and mixed evenly to obtain a modified aluminum silicate gelling liquid, and then the modified aluminum silicate gelling liquid is filled into the mold, a pressure of 0.18MPa is applied to it, and it is cured at 286°C for 2h. After curing, it is demolded, polished and cut to obtain a 50mm composite core layer 2.
[0039] Example 10 A Titanite slab, which is different from Example 1 in that, in the preparation of the composite core layer in step A2, the thermal insulation cotton is cut into a specification of 60mm*50mm*5mm, two pieces are selected and stacked and laid flat in a predetermined mold, and pre-pressed at 0.2MPa, and then the modified aluminum silicate gelling material prepared in Preparation Example 1 is added to a 0.6% aqueous solution of methacryloxysilane and mixed evenly to obtain a modified aluminum silicate gelling liquid, and then the modified aluminum silicate gelling liquid is filled into the mold, a pressure of 0.18MPa is applied to it, and it is cured at 286°C for 2h. After curing, it is demolded, polished and cut to obtain a 10mm composite core layer 2.
[0040] The Titanite slabs prepared in Examples 9-10 were sampled and performance tested according to the above test standards. The test results are shown in the following table.
[0041] Table: Performance test results of Examples 9-10 As can be seen from the above table, the flatness of the Titanite plate sample prepared in Example 9 is slightly reduced, and a small amount of degumming occurs, while the flatness of Example 10 is excellent, and there is no degumming phenomenon, but the flame retardant grade is reduced by one grade; The thickness of the composite core layer 2 of Example 1 is 30 mm, while the thickness of the composite core layer 2 of Example 9 is increased to 50 mm, which may lead to uneven internal heat transfer during the curing process, especially in the thicker part, which may lead to incomplete curing or uneven internal stress, thereby affecting the flatness and may cause debonding. The thickness of the composite core layer 2 of Example 10 is reduced to 10 mm. Although the flatness is excellent and there is no debonding, the thinner composite core layer 2 may reduce the thermal stability and flame retardancy of the material, so the flame retardant grade is reduced; Although all embodiments use polyurethane elastic glue for bonding and curing, the change in the thickness of the composite core layer 2 may require different curing conditions. A thicker composite core layer 2 may require a longer curing time and a higher temperature to ensure complete internal curing, otherwise the internal uncured portion may affect the overall performance. In addition, the modified aluminosilicate cementitious material used in the composite core layer 2 may have a specific curing shrinkage rate. When the composite core layer 2 is thicker, the shrinkage stress generated during the curing process may be greater, resulting in a decrease in flatness and debonding. A thinner composite core layer 2 has a smaller shrinkage stress.
[0042] Comparative Example 1 A Titanite slab is different from Example 1 in that the preparation method of the modified aluminosilicate cementitious material used in the preparation of the composite core layer in step A2 is different. In the preparation step S1 of the modified aluminosilicate cementitious material, citric acid accounting for 1% of the total weight of the mixed liquid is directly added, that is, the mixture is not slowly added while stirring.
[0043] Comparative Example 2 A Titanite slab differs from Example 1 in that the preparation method of the modified aluminosilicate cementitious material used in the preparation of the composite core layer in step A2 is different, and in the preparation step S1 of the modified aluminosilicate cementitious material, an equal amount of nano-alumina with an average particle size of 10-50 nanometers is used to replace the nano-whisker cellulose.
[0044] Comparative Example 3 A Titanite slab is different from Example 1 in that the preparation method of the modified aluminosilicate cementitious material used in the preparation of the composite core layer in step A2 is different, and an equal amount of isooctyl acrylate is used instead of 2-methoxyethyl acrylate in the preparation step S1 of the modified aluminosilicate cementitious material.
[0045] The Titanite slabs prepared in Comparative Examples 1-3 were selected and their performance was tested according to the above-mentioned test standards. The test results are shown in the following table.
[0046] Table: Comparative Examples 1-3 Performance Test Results It can be seen from the above table that the flatness of the Titanite slabs prepared by Comparative Examples 1-3 decreased to varying degrees, especially Comparative Examples 2 and 3, which had the largest decrease. Degumming occurred in Comparative Examples 1 and 3, and the flame retardant grade dropped by one level compared with Example 1.
[0047] In the preparation step S1 of the modified aluminosilicate gelling material, citric acid is added directly instead of being slowly added while stirring, which may cause uneven distribution of citric acid in the mixed liquid, resulting in local over-high or over-low concentration, thereby affecting the uniformity and performance of the modified aluminosilicate gelling material. The uneven modified material may cause uneven internal structure of the composite core layer 2, affecting its flatness and mechanical properties, and may even cause degumming, and also affect the flame retardant properties; nano-alumina with an average particle size of 10-50 nanometers is used to replace nano-whisker cellulose. Nano-alumina and nano-whisker cellulose differ in structure and properties. The introduction of nano-alumina may change the microstructure and properties of the composite core layer 2, thereby affecting the flatness and mechanical properties of the composite core layer 2, and may also have a certain impact on the interface compatibility between the composite core layer 2 and the polyurethane elastic glue, resulting in degumming.
[0048] In addition, if isooctyl acrylate is used as a substitute, the performance of the modified aluminosilicate gelling material may be changed, and this change may affect the bonding performance between the composite core layer 2 and the polyurethane elastic adhesive, as well as the flame retardant performance of the composite core layer 2.
[0049] The combination of aluminosilicate, nano whisker cellulose and 2-methoxyethyl acrylate shows significant advantages in Titanite. The nano whisker cellulose ensures the high flatness and uniform thickness of the composite core layer 2 with its uniform distribution and strong viscosity. At the same time, the stability of aluminosilicate ensures that the composite core layer 2 is not easily deformed or damaged during long-term use. The addition of 2-methoxyethyl acrylate improves the interface compatibility of the composite material, reduces stress concentration, and further improves the flatness. In addition, the high thermal stability of aluminosilicate and the enhancement of density and mechanical strength by nanowhisker cellulose together improve the flame retardant properties of the composite material. Although 2-methoxyethyl acrylate is an organic compound, it combines well with inorganic materials and does not reduce the overall flame retardant properties. More importantly, the additive significantly improves the bonding properties of the composite material. Combined with the strong viscosity of nanowhisker cellulose and the stability of aluminosilicate, a strong bond between the composite core layer 2 and the polyurethane elastic adhesive is ensured, thereby achieving a no-debonding effect and ensuring the long-term stability of the entire Titan rock board.
[0050] The above are all modifications without creative contribution or solutions that obviously constitute technical inspiration that can be made to the present embodiment as needed by technical personnel in this field after reading this specification, but they should be protected by patent law as long as they are within the scope of the claims of this application.
Claims
1. Titan rock plate, characterized in that: It comprises a calcium silicate board layer (1), a composite core layer (2), a calcium silicate board layer (1), an A2-grade fireproof core material (3) and a silk aluminum skin layer (5) which are arranged in sequence; The composite core layer (2) is formed by composite integration of modified aluminosilicate gelling material and thermal insulation cotton; The raw materials for preparing the modified aluminosilicate gelling material include the following components in weight fractions: 60-80 parts of aluminosilicate, 3-6 parts of nano whisker cellulose, and 5-10 parts of 2-methoxyethyl acrylate, and are prepared by the following preparation method: S1, adding aluminosilicate, nano whisker cellulose and 2-methoxyethyl acrylate to a methanol aqueous solution, slowly adding citric acid dropwise while stirring, and mixing well to obtain a mixed solution A; S2, adjusting the pH and temperature of the mixed solution A obtained in S1, and cooling after continuous stirring to obtain a viscous mixture B; S3, drying the viscous mixture B obtained in S2, and grinding it to obtain a modified aluminosilicate gelling material with a certain particle size distribution.
2. The Titanite plate according to claim 1, characterized in that: The wire-aluminum skin layer (5) is formed by bonding wire-aluminum skins.
3. The Titanite plate according to claim 1, characterized in that: The calcium silicate board layer (1) and the composite core layer (2), the composite core layer (2) and the A2-grade fireproof core material (3), and the A2-grade fireproof core material (3) and the aluminum skin layer (5) are bonded by polyurethane elastic adhesive, and the polyurethane elastic adhesive is cured to form a bonding layer (4).
4. The Titanite plate according to claim 1, characterized in that: An anchor bolt (21) is arranged on the composite core layer (2), the head of the anchor bolt (21) is pre-buried in the composite core layer (2), and the screw rod of the anchor bolt (21) passes through the composite core layer (2) and the calcium silicate board layer (1) in sequence.
5. The Titanite plate according to claim 1, characterized in that: The side of the A2-grade fireproof core material (3) is provided with a stainless steel fastener (31) for connection and fixation with the wall.
6. The method for preparing the Titanite slab according to any one of claims 1 to 5, characterized in that: The method comprises the following preparation steps: A1, preparation of calcium silicate board layer (1): the calcium silicate board is pretreated, and then the calcium silicate board layer (1); A2, preparation of the composite core layer (2): laying the thermal insulation cotton in a predetermined mold, pre-pressing it first, then adding the modified aluminum silicate gelling material to a 0.6wt% aqueous solution of methacryloxysilane and mixing them evenly to obtain a modified aluminum silicate gelling liquid, then filling the modified aluminum silicate gelling liquid into the mold, applying appropriate pressure, demoulding after curing, and performing subsequent processing operations to obtain a composite core layer (2); Preparation of A3 and A2 grade fireproof core material (3): molten glass fiber is mixed with aluminum hydroxide and phosphate and then filled into a mold, and pressed and molded at the same time, and then post-processed after cooling and molding; A4. Assembly: polyurethane elastic glue is applied on the surface of the calcium silicate board layer (1), the A2-class fireproof core material (3) and the composite core layer (2), and then the wire aluminum skin is attached to the A2-class fireproof core material (3) to form a wire aluminum skin layer (5). Then, a connection hole is opened on the composite core layer (2) and a stainless steel fastener (31) is installed on the side of the A2-class fireproof core material (3), and an anchor bolt (21) is inserted into the connection hole. The calcium silicate board layer (1), the wire aluminum skin layer (5), the A2-class fireproof core material (3) and the composite core layer (2) are bonded together, and appropriate pressure is applied. After solidification, the Titanite board is obtained.
7. The method for preparing the Titanite slab according to claim 6, characterized in that: The curing temperature of A2 is 260-290°C.
8. The method for preparing the Titanite slab according to claim 6, characterized in that: The post-processing operation in A3 includes one or more of surface cleaning, activation treatment, and cutting.