Vacuum control system and control method for smelting magnesium and co-producing calcium carbide through carbon thermal method

Through the vacuum control system combining Roots pump, slide valve pump, variable frequency water ring pump and electric control valve, the problem of vacuum control in calcium carbide co-production by carbon-heat method is solved, and the collection rate and production safety of magnesium are improved , and realize the production of high purity magnesium and high value added calcium carbide.

CN118980260APending Publication Date: 2024-11-19BAOSTEEL METAL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411039695.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-12-29
Filing Date
2024-07-31
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing vacuum system cannot meet the specific requirements of vacuum degree at different reaction stages of magnesium-based co-production of calcium carbide by carbon-thermal magnesium, resulting in contact between magnesium vapor and CO, reducing the magnesium collection rate and purity, and posing safety hazards.

Method used

Using a vacuum control system combining Roots pump, slide valve pump, variable frequency water ring pump and electric control valve, the vacuum degree in the reactor is accurately controlled at different reaction stages by automatically adjusting the frequency of variable frequency water ring pump and the opening of the electric control valve. Avoid contact between magnesium vapor and CO within the required range.

Benefits of technology

It improves the collection rate and production safety of magnesium, realizes the production of high-purity magnesium and high value-added calcium carbide by-products, reduces the complexity of the condensation device, and avoids waste slag emissions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118980260A_ABST
    Figure CN118980260A_ABST
Patent Text Reader

Abstract

According to the vacuum control system and method for smelting magnesium and co-producing calcium carbide through the carbon thermal method, a variable-frequency water ring pump and an automatic control valve are additionally arranged and are connected with a slide valve pump in parallel to form the vacuum control system, and through adjustment of a variable-frequency vacuum pump and the automatic control valve, the requirements of different reaction stages for the vacuum degree are precisely controlled; and the pressure in the reaction furnace in different reaction stages can be automatically adjusted in a required range. According to the invention, different requirements of two different reaction stages on the vacuum degree can be met, contact between magnesium steam and CO can be effectively avoided, the collection rate of magnesium is greatly improved, the production safety is improved, and meanwhile, a calcium carbide byproduct with high utilization value is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of nonferrous metal metallurgy, and in particular to a vacuum control system and a control method for carbothermic magnesium smelting and co-production of calcium carbide. Background Art

[0002] At present, 90% of magnesium in industry is smelted by the Pidgeon process (silicothermic process). The Pidgeon process is to reduce calcined white with 75% ferrosilicon to obtain magnesium under the conditions of 1200℃ and vacuum degree less than 13Pa. The lower the vacuum degree, the more conducive to the reduction reaction. The vacuum system solution used in industry is to use a direct-connected pump and a diffusion pump to connect and operate at rated power to achieve the ultimate vacuum degree. The Pidgeon process will generate a large amount of dicalcium silicate while generating magnesium. There is currently no large-scale treatment method for the dicalcium silicate, which is usually landfilled. In addition, the Pidgeon process has high energy consumption, high carbon dioxide emissions, low mechanization and automation, high labor intensity of workers, and a relatively poor working environment. As people pay more and more attention to environmental protection, the Pidgeon process has been included in the restricted list since 2011.

[0003] The carbothermal method uses carbon as a reducing agent to reduce calcined magnesite under high temperature and high vacuum to obtain magnesium vapor and CO. The carbothermal method uses a carbonaceous reducing agent, which can greatly reduce the smelting cost compared to the Pidgeon method using ferrosilicon as a reducing agent. The produced CO has a higher purity and can be used as a fuel. There is no reduction slag, and it is significantly more environmentally friendly than the Pidgeon method. However, when the magnesium vapor and CO mixed gas are cooled together, a reverse reaction Mg(g)+CO(g)=MgO(s)+C(s) will occur, which greatly reduces the collection rate and purity of magnesium. When the reverse reaction is suppressed by quenching, magnesium powder will inevitably be produced. At high temperatures, magnesium powder is very likely to explode when it encounters air, posing a serious safety hazard.

[0004] Chinese patent CN202080087519.1 discloses a method for carbon thermal magnesium smelting and co-production of calcium carbide, by controlling the temperature and vacuum degree, so that the temperature and vacuum degree have a certain matching relationship: 11lg 2 P+71lgP+1210℃ <T<98lg 2 P-129lgP+1300℃. The reaction is divided into two stages. In the first stage, CaMgO 2 (s)+CaC 2 (s)=Mg(g)+2CaO(s)+2C(s), in the second stage, CaO(s)+3C(s)=CaC 2 (s)+CO(g) to produce magnesium vapor and CO gas respectively, avoiding the contact between magnesium vapor and CO from the source, thereby reducing the complexity of the condensation device, greatly improving the magnesium collection rate, and obtaining calcium carbide as a by-product with high utilization value.

[0005] However, if a traditional silicon thermal vacuum system is used to control the vacuum degree of the reaction device in Chinese patent CN202080087519.1, that is, the vacuum pump is operated at a fixed limit power to achieve a maximum constant vacuum degree, the vacuum degree cannot be controlled within a specific range matching the temperature at different reaction stages, and the requirements of a carbon thermal method for magnesium smelting and co-production of calcium carbide disclosed in Chinese patent CN202080087519.1 cannot be met.

[0006] Therefore, developing a new vacuum system and how to operate the vacuum system to meet the different requirements of the vacuum degree of the reaction device at each stage are issues that need to be urgently addressed. Summary of the invention

[0007] The object of the present invention is to provide a vacuum control system and a control method for carbothermic magnesium smelting and co-production of calcium carbide, which can meet the different requirements of the process for vacuum degree in different reaction stages, effectively avoid the contact between magnesium vapor and CO, reduce the complexity of the condensation device, greatly improve the collection rate of magnesium and improve production safety, and at the same time obtain a calcium carbide by-product with high added value without waste slag discharge.

[0008] To achieve the above purpose, the technical solution of the present invention is as follows:

[0009] A vacuum control system for carbothermal magnesium smelting and calcium carbide co-production, comprising:

[0010] A reaction furnace is provided with an air inlet and an air outlet; the air inlet is connected to the gas storage tank through an air inlet pipeline, and an air charging valve is provided on the air inlet pipeline;

[0011] A Roots pump is connected to the gas outlet of the reactor through a gas outlet pipeline, a Roots pump control valve is provided on the gas outlet pipeline, and a baffle valve and an electric control valve are sequentially provided on the outlet pipeline of the Roots pump;

[0012] A slide valve pump, connected to the outlet pipeline of the electric control valve through a pipeline and an upper slide valve pump control valve;

[0013] The variable frequency water ring pump is connected to the outlet pipe of the electric control valve through the pipeline and the variable frequency water ring pump control valve on it;

[0014] The controller is electrically connected to the reactor, the charging valve, the Roots pump control valve, the baffle valve, the electric control valve, the slide valve pump control valve, and the variable frequency water ring pump control valve.

[0015] The present invention also provides a vacuum degree control method using the system. During the first stage of magnesium smelting, the baffle valve is first opened, the Roots pump control valve, the slide valve pump control valve and the slide valve pump are opened, and after the vacuum degree in the reaction furnace is pumped to the limit vacuum degree of the slide valve pump, the Roots pump is opened to pump the vacuum degree in the reaction furnace to the limit vacuum degree (about 10Pa), the slide valve pump, the slide valve pump control valve and the Roots pump are closed, the variable frequency water ring pump and the variable frequency water ring pump control valve are opened, and the charging valve is opened at the same time, argon is charged into the reaction furnace until the vacuum degree required for the first stage reaction is 10 to 5000Pa, the charging valve is closed, and the first stage reaction is carried out;

[0016] After the first stage reaction is completed, the charging valve is opened, and argon gas is continuously charged into the reactor until the vacuum required for the second stage reaction reaches 5000-15000Pa, and the charging valve is closed;

[0017] The required vacuum degree in the first and second stage reaction processes is achieved by automatically adjusting the frequency of the variable frequency water ring pump or by automatically adjusting the frequency of the variable frequency water ring pump and setting the opening size of the electric control valve. When the vacuum degree in the reactor exceeds the set value, the frequency of the variable frequency water ring pump and the opening of the electric control valve are increased. Conversely, when the vacuum degree in the reactor is lower than the set value, the frequency of the variable frequency water ring pump and the opening of the electric control valve are reduced, so as to accurately control and maintain the vacuum degree in the reactor within the set range.

[0018] Preferably, the temperature required for the first stage and the second stage reaction is T, in °C, which satisfies the following relationship: 11lg 2 P+71lgP+1210<T<98lg 2 P-129lgP+1300; where P is the vacuum degree in the reactor, unit: Pa.

[0019] The control system of the present invention adopts a Roots pump, a sliding valve pump, a variable frequency water ring pump and an electric control valve to form a vacuum control system for use with a supporting reactor, and can control the vacuum degree to meet different pressure requirements in two reaction stages.

[0020] The vacuum degree values ​​that need to be controlled in the reactor in the two reaction stages are set on the overall control structure, and are achieved by automatically adjusting the frequency of the variable frequency water ring pump or automatically adjusting the frequency of the variable frequency water ring pump and setting the opening size of the electric control valve. When the vacuum degree in the reactor exceeds the set value, the frequency of the variable frequency water ring pump and the opening of the electric control valve are increased. Conversely, when the vacuum degree in the reactor is lower than the set value, the frequency of the variable frequency water ring pump and the opening of the electric control valve are reduced, so as to accurately control and maintain the vacuum degree in the reactor within the set range, and realize automatic adjustment of the vacuum degree range in the reactor in different reaction stages.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] The present invention forms a vacuum control system by adding a variable frequency vacuum pump (variable frequency water ring pump) and an automatic control valve in parallel with a sliding valve pump. Through the adjustment of the variable frequency vacuum pump and the automatic control valve, the requirements for the vacuum degree in different reaction stages are accurately controlled, and the vacuum degree in the reactor in different reaction stages is automatically adjusted within the required range.

[0023] However, existing vacuum control systems all operate at the rated maximum power of Roots pumps and sliding valve pumps (i.e., pump to the ultimate vacuum degree), and are unable to stably control the vacuum degree within a range above the ultimate vacuum degree.

[0024] The system of the present invention can realize the control of vacuum degree and temperature. The reaction is divided into two stages. In the first stage, CaMgO 2 (s)+CaC 2 (s)=Mg(g)+2CaO(s)+2C(s), in the second stage, CaO(s)+3C(s)=CaC 2 (s)+CO(g) to produce magnesium vapor and CO gas respectively, thus avoiding the contact between magnesium vapor and CO from the source, thereby avoiding the occurrence of reverse reaction, reducing the oxidation of magnesium vapor, and greatly improving the collection rate of magnesium. The collection rate of magnesium is increased by about 10% compared with the existing technology. In theory, 100% of magnesium vapor can be collected; at the same time, production safety is also improved, and calcium carbide, a by-product with high utilization value, is obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 The figure is a schematic diagram of a vacuum control system for carbothermal magnesium smelting and co-production of calcium carbide according to an embodiment of the present invention.

[0026] Figure 2 This is a microscopic morphology photograph of magnesium obtained in Example 1 of the present invention.

[0027] Figure 3 This is the EDS energy spectrum analysis result of magnesium obtained in Example 1 of the present invention.

[0028] Figure 4 This is a microscopic morphology photograph of magnesium obtained in Example 2 of the present invention.

[0029] Figure 5 This is the EDS energy spectrum analysis result of magnesium obtained in Example 2 of the present invention. DETAILED DESCRIPTION

[0030] The present invention will be further described below in conjunction with the embodiments and drawings.

[0031] See also Figure 1 The vacuum control system for carbothermal magnesium smelting and calcium carbide co-production according to the present invention comprises:

[0032] A reaction furnace 1 is provided with an air inlet and an air outlet; the air inlet is connected to a gas storage tank 2 through an air inlet pipeline, and an air charging valve F1 is provided on the air inlet pipeline;

[0033] A Roots pump 3 is connected to the gas outlet of the reactor 1 through a gas outlet pipeline, on which a Roots pump control valve F2 is provided, and a baffle valve F3 and an electric control valve F4 are sequentially provided on the outlet pipeline of the Roots pump 3;

[0034] Sliding valve pump 4, connected to the outlet pipeline of electric control valve F4 through the pipeline and the sliding valve pump control valve F5 on it;

[0035] The variable frequency water ring pump 5 is connected to the outlet pipe of the electric control valve F4 through the pipeline and the variable frequency water ring pump control valve F6 on it;

[0036] The controller 6 , the reactor 1 , the charging valve F1 , the Roots pump control valve F2 , the baffle valve F3 , the electric control valve F4 , the slide valve pump control valve F5 , and the variable frequency water ring pump control valve F6 are all electrically connected to the controller 6 .

[0037] Example 1

[0038] During the first stage of magnesium smelting, the baffle valve is opened, the Roots pump control valve, the slide valve pump and the slide valve pump control valve are opened, and after the vacuum degree in the reactor is evacuated to the limit vacuum degree of the slide valve pump of about 3000Pa, the Roots pump is opened, and when the vacuum degree of the reactor is evacuated to the limit vacuum degree of 10Pa or less, the slide valve pump, the slide valve pump control valve and the Roots pump are closed, the variable frequency water ring pump and the variable frequency water ring pump control valve are opened, and the charging valve is opened at the same time, argon is charged to the vacuum degree of 2000Pa required for the first stage reaction, and then the temperature is increased to the temperature of 1600°C required for the first stage reaction, and the temperature is kept to react; during the reaction, the upper limit of the opening of the electric control valve is set on the controller, and when the vacuum degree in the reactor is lower than 2000Pa, the opening of the electric control valve increases, and when the vacuum degree in the reactor is higher than 2000Pa, the opening of the electric control valve decreases;

[0039] After the first stage reaction is completed, the system automatically opens the gas cylinder and fills in argon to the vacuum degree of 8000Pa required for the second stage smelting calcium carbide reaction, and continues to increase the temperature to the temperature of 1700℃ required for the second stage reaction, keeps warm, and reacts; during the second stage reaction, when the vacuum degree in the reactor is lower than 8000Pa, the opening of the electric control valve increases, and when the vacuum degree in the reactor is higher than 8000Pa, the opening of the electric control valve decreases.

[0040] Ultimately, the contact between magnesium vapor and CO is effectively avoided, the magnesium collection rate is increased, the production safety is improved, and higher-purity magnesium and by-product calcium carbide are obtained.

[0041] In the first stage of magnesium smelting, the magnesium smelting reduction rate is measured by the weight loss of the reaction materials and the residual content of magnesium element is measured by ICP to calculate the magnesium smelting reduction rate. For specific data, see Table 1:

[0042] Table 1

[0043]

[0044] As can be seen from Table 1, the reduction rate measured by weight loss is basically consistent with the reduction rate measured by ICP, indicating that only the reaction of generating magnesium vapor occurred in the first stage, and no CO gas was generated; if the weight loss is significantly greater than the data measured by ICP, it means that CO gas is generated.

[0045] The gas emission of calcium carbide obtained by measurement in the second stage is shown in Table 2.

[0046] Table 2

[0047]

[0048] As can be seen from Table 2, the gas evolution of the calcium carbide obtained in the second stage proves that the calcium carbide obtained by this method has reached the high-quality grade and meets the standard for sale as a commodity.

[0049] Finally, the magnesium microstructure and EDS spectrum are as follows: Figure 2 and Figure 3 As shown, from Figure 2 and Figure 3 As shown, it is proved that the obtained magnesium metal has high purity and is free of impurities.

[0050] Example 2

[0051] During the first stage of magnesium smelting, the baffle valve is opened, the Roots pump control valve, the slide valve pump and the slide valve pump control valve are opened, and after the vacuum degree in the reactor is evacuated to the limit vacuum degree of the slide valve pump of about 3000Pa, the Roots pump is opened, and when the vacuum degree of the reactor is evacuated to the limit vacuum degree of 10Pa or less, the slide valve pump, the slide valve pump control valve and the Roots pump are closed, the variable frequency water ring pump and the variable frequency water ring pump control valve are opened, and the charging valve is opened at the same time, argon is charged to the vacuum degree of 1000Pa required for the first stage reaction, and then the temperature is increased to the temperature of 1550°C required for the first stage reaction, and the temperature is kept to react; during the reaction, the upper limit of the opening of the electric control valve is set on the controller, and when the vacuum degree in the reactor is lower than 1000Pa, the opening of the electric control valve increases, and when the vacuum degree in the reactor is higher than 1000Pa, the opening of the electric control valve decreases;

[0052] After the first stage reaction is completed, the system automatically opens the gas storage bottle and fills in argon to the vacuum degree of 10000Pa required for the second stage smelting calcium carbide reaction, and continues to raise the temperature to the temperature of 1750℃ required for the second stage reaction, keeps warm, and reacts; during the second stage reaction, when the vacuum degree in the reactor is lower than 10000Pa, the opening degree increases, and when the vacuum degree in the reactor is higher than 10000Pa, the opening degree of the electric control valve decreases.

[0053] Ultimately, the contact between magnesium vapor and CO is effectively avoided, the magnesium collection rate is increased, the production safety is improved, and higher-purity magnesium and by-product calcium carbide are obtained.

[0054] In the first stage of magnesium smelting, the magnesium smelting reduction rate is calculated by measuring the weight loss of the reaction materials and the residual content of magnesium element by ICP. For specific data, see Table 3:

[0055] Table 3

[0056]

[0057]

[0058] It can be seen from Table 3 that the reduction rate measured by weight loss is basically consistent with the reduction rate measured by ICP, indicating that only the reaction of generating magnesium vapor occurred in the first stage, and no CO gas was generated; if the weight loss is significantly greater than the data measured by ICP, it means that CO gas is generated.

[0059] The gas emission of calcium carbide obtained by measurement in the second stage is shown in Table 4.

[0060] Table 4

[0061]

[0062] As can be seen from Table 4, the gas evolution of the calcium carbide obtained in the second stage proves that the calcium carbide obtained by this method has reached the high-quality grade and meets the standard for sale as a commodity.

[0063] Finally, the magnesium microstructure and EDS spectrum are as follows: Figure 4 and Figure 5 As shown, from Figure 4 and Figure 5 As shown, it is proved that the obtained magnesium metal has high purity and is free of impurities.

Claims

1. A vacuum control system for carbothermal magnesium smelting and co-production of calcium carbide, characterized in that: It includes a reaction furnace, which is provided with an air inlet and an air outlet; the air inlet is connected to a gas storage tank through an air inlet pipeline, and the air inlet pipeline is provided with an air charging valve; A Roots pump is connected to the gas outlet of the reactor through a gas outlet pipeline, a Roots pump control valve is provided on the gas outlet pipeline, and a baffle valve and an electric control valve are sequentially provided on the outlet pipeline of the Roots pump; A slide valve pump, connected to the outlet pipeline of the electric control valve through a pipeline and an upper slide valve pump control valve; The variable frequency water ring pump is connected to the outlet pipe of the electric control valve through the pipeline and the variable frequency water ring pump control valve on it; The controller is electrically connected to the reactor, the charging valve, the Roots pump control valve, the baffle valve, the electric control valve, the slide valve pump control valve, and the variable frequency water ring pump control valve.

2. A vacuum degree control method using the system as claimed in claim 1, characterized in that: When smelting magnesium, first open the baffle valve, open the Roots pump control valve, the slide valve pump control valve and the slide valve pump, and after the vacuum degree in the reaction furnace is pumped to the limit vacuum degree of the slide valve pump, open the Roots pump to pump the vacuum degree in the reaction furnace to below the limit vacuum degree, close the slide valve pump, the slide valve pump control valve and the Roots pump, open the variable frequency water ring pump and the variable frequency water ring pump control valve, and open the charging valve at the same time, fill the reaction furnace with argon gas to the vacuum degree of 10-5000Pa required for the first stage reaction, close the charging valve, and carry out the first stage reaction; After the first stage reaction is completed, the charging valve is opened, and argon gas is continuously charged into the reactor until the vacuum required for the second stage reaction reaches 5000-15000Pa, and the charging valve is closed; The required vacuum degree in the first and second stage reaction processes is achieved by automatically adjusting the frequency of the variable frequency water ring pump or by automatically adjusting the frequency of the variable frequency water ring pump and setting the opening size of the electric control valve. When the vacuum degree in the reactor exceeds the set value, the frequency of the variable frequency water ring pump and the opening of the electric control valve are increased. Conversely, when the vacuum degree in the reactor is lower than the set value, the frequency of the variable frequency water ring pump and the opening of the electric control valve are reduced, so as to accurately control and maintain the vacuum degree in the reactor within the set range.

3. The vacuum degree control method according to claim 2, characterized in that: The temperature required for the first and second stage reactions is T, in °C, which satisfies the following relationship: 11lg 2 P+71lgP+1210<T<98lg 2 P-129lgP+1300; where P is the vacuum degree in the reactor, unit: Pa.