Titanium-based composite material EBSD test sample preparation method
Through the combination of mechanical polishing and tri-ion beam polishing, the problem of low calibration rate of EBSD test of titanium-based composite materials is solved, and efficient sample preparation and fatigue crack analysis are achieved, which is suitable for samples after high stress and fatigue testing.
Patent Information
- Application Number
- CN202411155799.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-19
AI Technical Summary
Titanium-based composite materials are difficult to prepare in EBSD tests, especially the electronic signal occlusion and oxidation caused by ceramic phase reinforcement, which makes the test calibration rate low and the internal high-stress samples difficult to accurately analyze.
Using a combination of mechanical polishing and tri-ion beam polishing, the sample surface is polished and anti-oxidation treatment is carried out before the tri-ion beam polishing, to control the polishing accuracy and parameters to ensure that the sample surface has no oxide layer and stress reduction.
The calibration rate of EBSD test is improved to 92% or above, ensuring the true morphological characteristics of the fatigue crack tip and the accuracy of crystal tissue analysis, and is suitable for samples after high stress and fatigue testing.
Smart Images

Figure CN118980701A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of material performance testing, and particularly relates to a method for preparing an EBSD testing sample of a titanium-based composite material. Background Art
[0002] Titanium-based composites have excellent room temperature and high temperature mechanical properties and have broad application prospects in the aerospace field. In recent years, with the continuous deepening of research on the mechanical properties and organizational evolution of titanium-based composites, the application of Electron Backscattered Diffraction (EBSD) technology in the characterization of texture, Schmidt factor, twin nucleation and crystallographic orientation relationship in titanium-based composites has become more and more extensive.
[0003] Titanium-based composite materials have the characteristics of high hardness and strong corrosion resistance of the hard ceramic phase. When the traditional titanium alloy electrolytic polishing technology is used to prepare EBSD test samples, the corrosion-resistant reinforcement will block the electronic signal, resulting in a low calibration rate of the surrounding matrix, and difficulty in collecting texture information and crystallographic orientation information. In addition, titanium-based composite materials have high metal activity and are prone to oxidation, while electron backscatter diffraction only occurs at a depth of tens of nanometers on the sample surface. Only when the sample surface is stress-free and has no oxide layer can better test characterization results be obtained. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing EBSD test samples of titanium-based composite materials, so as to solve the problem that EBSD test samples of titanium-based composite materials are difficult to prepare and the prepared samples cannot meet the test requirements.
[0005] The present invention is achieved through the following technical solutions: The method for preparing a titanium-based composite material EBSD test specimen comprises the following steps: S01. Mechanically polish the cut sample to polish the test surface of the sample to a mirror surface; S02, cleaning and drying the polished sample; S03. Perform triple ion beam polishing on the test surface of the sample, including: S031, rough polishing: polishing for 20min-80min at a voltage of 5-8kV, and the rotation angle of the sample stage during the rough polishing is 8°-12°; S032, fine polishing: polishing at a voltage of 3-5kV for 30min-100min, and the rotation angle of the sample stage during the rough polishing is 3°-6°.
[0006] As a further improvement to the above technical solution, in step S01, the step of mechanically polishing the sample includes: S011. Use sandpaper of different mesh sizes to polish the test surface respectively; S012. Rough polishing of the test surface is performed using a chromium oxide polishing liquid, the mass fraction of the chromium oxide polishing liquid is 1-5%, the solvent is deionized water, the speed of the polishing machine is 200r / min-1000r / min, and the sample test surface is continuously cooled during the rough polishing process; S013. Use diamond polishing pastes of different specifications to polish the test surfaces respectively, and polish the test surfaces of the samples to a surface roughness Ra ≤ 0.8 μm.
[0007] As a further improvement to the above technical solution, in step S011, sandpaper with gradually increasing mesh sizes is used to polish the test surface, and the mesh size of the sandpaper is 120-2000 meshes.
[0008] As a further improvement to the above technical solution, the rotation speed of the grinding and polishing machine in step S012 is 200r / min-600r / min.
[0009] As a further improvement to the above technical solution, in step S013, diamond polishing paste with gradually increasing mesh sizes is used to fine-polish the test surface, and the specification of the diamond polishing paste is W5.0-W1.5.
[0010] As a further improvement to the above technical solution, in step S02, the sample is immersed in anhydrous ethanol and ultrasonically cleaned for 5-15 minutes. After cleaning and drying the sample, the test surface is covered with an antistatic blue film.
[0011] As a further improvement to the above technical solution, the voltage of the rough polishing treatment in step S031 is 5 kV, the sample stage rotation angle is 10.5°, and the treatment time is 30 min; In step S032, the voltage of the fine polishing treatment is 4.5 kV, the rotation angle of the sample stage is 4.5°, and the treatment time is 45 minutes.
[0012] As a further improvement to the above technical solution, when the test surface of the sample is subjected to triple ion beam polishing, the crack tip on the sample is located at the center of the sample stage.
[0013] As a further improvement to the above technical solution, the sample is a titanium-based composite material including a titanium alloy matrix and a ceramic phase reinforcement.
[0014] As a further improvement to the above technical solution, the sample is a titanium-based composite material having an internal stress of 300-900 MPa after deformation or after fatigue testing.
[0015] Compared with the prior art, the present invention has the following beneficial effects: The preparation method of the present invention is aimed at titanium-based composite materials, especially titanium-based composite materials with a titanium alloy matrix and a ceramic phase reinforcement, and samples with high stress inside, such as large deformation after rolling, stretching, etc., or after fatigue testing, and the problems of difficult sample preparation and low sample calibration rate. A method combining mechanical polishing with three-ion beam polishing is adopted to control the polishing accuracy of each stage, and the process and parameters of the three-ion beam polishing are controlled to ensure the preparation quality of the sample. The sample EBSD test calibration rate can reach 92% or above.
[0016] The method of the present invention can effectively reduce the internal stress inside the titanium-based composite material, making it suitable for testing samples after fatigue crack growth tests, can well ensure the true morphological characteristics of the crack tip, and realize accurate analysis of the fatigue crack crystal structure.
[0017] The method of the present invention performs anti-oxidation treatment on the test surface of the sample before triple ion beam polishing, which can further improve the preparation quality of the sample.
[0018] The method of the present invention has important practical significance for the texture analysis, plastic deformation mechanism analysis and orientation analysis of the reinforcement and the matrix of titanium-based composite materials, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0020] Figure 1 Schematic diagram of the characterization of the tissue characteristics of the sample prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0021] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments.
[0022] For titanium-based composite materials, especially those with a titanium alloy matrix and ceramic phase reinforcements, and which have high stress inside, such as large deformation after rolling, stretching, or fatigue testing, the samples obtained by the existing sample preparation method have the problem of low calibration rate during the test process due to the influence of factors such as ceramic phase reinforcements and surface stress.
[0023] In view of the characteristics of this material, the test sample preparation method in this embodiment can realize the rapid preparation of the test sample and can well solve the problem of ceramic phase reinforcement and high stress on the sample surface, and includes the following steps: 1) Sample cutting The test samples are cut by wire cutting. Good cooling conditions should be maintained during the processing to minimize the impact on the sample structure.
[0024] The size of the cut samples should be controlled within 30mm×30mm, and the thickness should be controlled within 10mm.
[0025] 2) Mechanical polishing The test surface of the sample was polished with 120 mesh, 400 mesh, 800 mesh, 1000 mesh, and 2000 mesh sandpaper in turn; Then, the sample is roughly polished on the polishing disk of the grinder and polisher using a chromium oxide polishing liquid; during the polishing process, the speed of the grinder and polisher is controlled at 200 r / min-1000 r / min, preferably 200 r / min-600 r / min, and the polishing surface is continuously cooled by water during the polishing process; The mass fraction of the chromium oxide polishing liquid used is 1-5%, and the rest is deionized water. Deionized water is used to keep the metallographic polishing cloth moist during the polishing process. During the polishing process, deionized water is used to clean the chromium oxide polishing liquid and metallographic polishing cloth remaining on the surface of the sample test surface; Finally, diamond polishing pastes with specifications of W5.0, W3.5, and W1.5 were used to polish the samples until the test surface of the samples was polished to a mirror finish with no obvious scratches on the surface. During the fine polishing process, when changing diamond polishing pastes of different specifications, the polishing cloth and sample used should be cleaned.
[0026] 3) Cleaning and drying Soak the mechanically polished sample in anhydrous ethanol, clean it in an ultrasonic cleaner at room temperature for 5-15 minutes, vibrate clean the sample, and use a hair dryer to dry the sample test surface; The test surface is then covered with an antistatic blue film to prevent oxidation of the test surface.
[0027] 4) Triple ion beam polishing The test surface of the sample is plane-polished using a triple ion beam polisher to obtain an EBSD test specimen; including: Rough polishing: polishing for 20-80 minutes at a voltage of 5-8kV, and the rotation angle of the sample stage during the rough polishing is 8°-12°; Fine polishing: Polishing is performed at a voltage of 3-5kV for 30min-100min, and the rotation angle of the sample stage during rough polishing is 3°-6°.
[0028] The calibration rate of the titanium-based composite material EBSD test specimen prepared by the above method and steps can reach more than 92%.
[0029] The features and performance of the present invention are further described in detail below in conjunction with specific embodiments.
[0030] Example 1 The test specimen used in this embodiment is a titanium-based composite material after a high-temperature fatigue crack growth test, and the following steps are included: 1) After high temperature fatigue crack growth test, the sample including the crack tip was cut by wire cutting. The sample size was 10 mm × 10 mm × 5 mm, and then metallographic hot mounting was performed in a fully automatic metallographic mounting machine.
[0031] 2) In the grinding and polishing machine, use 120 mesh, 400 mesh, 800 mesh, 1000 mesh, and 2000 mesh sandpaper to grind the sample in sequence. Use cooling water to cool the sample during the grinding process until there are no obvious coarse scratches on the test surface of the sample, and only fine scratches with the same direction can be observed; Then, the sample was roughly polished with a chromium oxide polishing liquid with a mass fraction of 5% to further reduce scratches on the sample test surface. The polishing time was 5 minutes. Continue to use diamond polishing pastes with specifications of W5.0, W3.5, and W1.5 for fine polishing, and clean the polishing cloth and sample test surface every time you change a polishing paste to prevent residual particles from affecting the sample surface; the polishing time is about 10 minutes, until the sample surface is in a bright mirror state, and the surface roughness of the sample test surface is Ra≤0.8μm.
[0032] 3) Place the sample in a 100 ml beaker and pour in anhydrous ethanol to immerse the sample, then use an ultrasonic cleaner to vibrate and clean for 15 minutes to prevent polishing liquid, water stains and debris from remaining in the fatigue crack; After vibration cleaning, use cold air from a hair dryer to dry the sample surface, and then cover the sample test surface with an antistatic blue film to prevent the sample surface from being scratched or oxidized.
[0033] 4) The test surface was plane-polished using a triple ion beam polisher, with the crack tip on the sample located at the center of the sample stage. The voltage for rough polishing was 5 kV, the sample stage rotation angle was 10.5°, and the processing time was 30 min; the voltage for fine polishing was 4.5 kV, the sample stage rotation angle was 4.5°, and the processing time was 45 min. After triple ion beam polishing, the crack tip of the sample presents a thin haze surface.
[0034] During EBSD testing, the haze area is observed.
[0035] Reference Figure 1 FE-SEM and Nova / NanoSEM 230 field emission scanning electron microscope were used to characterize and analyze the titanium-based composite materials prepared above. It can be seen from the figure that the orientation imaging effect of the inverse pole figure is very good. The calibration rate of titanium-based composite materials including high-temperature fatigue cracks reached 92%, with clear contrast. The cracks inside the TiC ceramic phase at the fatigue crack tip are clearly visible. The single cross-section trace method can be used to analyze the cleavage surface of TiC particles at the high-temperature fatigue crack tip, and the pole figure can be used to analyze the orientation relationship between TiC and the surrounding Ti matrix.
[0036] Example 2 In this embodiment, when three ion beams are used for polishing, the polishing parameters used are: the voltage of the rough polishing is 8 kV, the sample stage tilt angle is 12°, and the processing time is 20 min; the voltage of the fine polishing is 3 kV, the sample stage tilt angle is 6°, and the processing time is 60 min; the other processing steps are the same as in Example 1.
[0037] Example 3 In this embodiment, when triple ion beam polishing is used, the polishing parameters used are: the voltage of the rough polishing is 6 kV, the sample stage tilt angle is 8°, and the processing time is 80 min; the voltage of the fine polishing is 5 kV, the sample stage tilt angle is 3°, and the processing time is 100 min; the other processing steps are the same as in Example 1.
[0038] Comparative Example 1 Conventional vibration polishing is used to replace the triple ion beam polishing process steps in Example 1, and the other processing steps are the same.
[0039] Comparative Example 2 Conventional electrolytic polishing is used to replace the triple ion beam polishing process steps in Example 1, and the other processing steps are the same.
[0040] Comparative Example 3 In this comparative example, when triple ion beam polishing was used, the polishing parameters used were: the voltage of the rough polishing was 8 kV, the sample stage tilt angle was 6°, and the processing time was 60 min; the voltage of the fine polishing was 4.5 kV, the sample stage tilt angle was 4.5°, and the processing time was 45 min; the other processing steps were the same as in Example 1.
[0041] Comparative Example 4 In this comparative example, when triple ion beam polishing was used, the polishing parameters used were: the voltage of the rough polishing was 5 kV, the sample stage tilt angle was 10.5°, and the processing time was 30 min; the voltage of the fine polishing was 2.5 kV, the sample stage tilt angle was 2.5°, and the processing time was 60 min; the other processing steps were the same as in Example 1.
[0042] In the above embodiments, the EBSD test calibration rate of the samples containing high-temperature fatigue extension cracks can reach 92%, and the contrast is clear, and the cracks inside the TiC ceramic phase at the fatigue crack tip are clearly visible.
[0043] In Comparative Example 1, the vibration-polished sample cannot reduce the internal stress at the fatigue crack tip and along the crack, so the calibration rate during EBSD test analysis is less than 50%, and accurate test information cannot be obtained; In Comparative Example 2, when electrolytic polishing is used for treatment, the cracks are corroded and deformed during the electrolytic process, resulting in the inability to truly restore the fatigue crack morphology and the inability to accurately analyze the crystallographic characteristics of fatigue crack propagation.
[0044] It can be seen from the above two comparative examples that, compared with the above-mentioned traditional polishing method, the method of the present invention avoids the corrosion of the test surface cracks caused by electrolytic polishing, can truly restore the fatigue crack morphology, and can effectively reduce the internal stress at the fatigue crack tip and along the crack, thereby improving the EBSD calibration rate of titanium-based composite materials.
[0045] In Comparative Examples 3 and 4, when only the polishing parameters of the rough polishing and the fine polishing in the triple ion beam polishing process were changed, it was found that the calibration rates of the EBSD tests of the samples decreased to a certain extent, at about 85% and 89%, respectively. This indicates that in addition to the combination of mechanical polishing and triple ion beam polishing used in the method of the present invention to ensure the preparation quality of the samples, the polishing parameters of the triple ion beam polishing treatment used also have a great influence on the preparation quality of the titanium-based composite materials.
[0046] In the description of the present invention, it should be noted that the terms "center", "up", "down", "left", "right", "vertical", "horizontal", "inside", "outside", etc. used to indicate the orientation or position relationship are based on the orientation or position relationship shown in the accompanying drawings, or are the orientation or position relationship commonly placed when the product of the invention is used. They are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0047] In addition, if the terms "horizontal" or "vertical" appear in the description of the present invention, it does not mean that the components are required to be absolutely horizontal or suspended, but can be slightly tilted. For example, "horizontal" only means that its direction is more horizontal than "vertical", and does not mean that the structure must be completely horizontal, but can be slightly tilted.
[0048] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification or equivalent change made to the above embodiment based on the technical essence of the present invention shall fall within the protection scope of the present invention.
Claims
1. A method for preparing a titanium-based composite material EBSD test sample, characterized in that: The following steps are involved: S01. Mechanically polish the cut sample to polish the test surface of the sample to a mirror surface; S02, cleaning and drying the polished sample; S03. Perform triple ion beam polishing on the test surface of the sample, including: S031, rough polishing; Polishing is performed at a voltage of 5-8kV for 20-80 minutes, and the rotation angle of the sample stage during the rough polishing is 8°-12°; S032, fine polishing: polishing at a voltage of 3-5kV for 30min-100min, and the rotation angle of the sample stage during the rough polishing is 3°-6°.
2. The method for preparing a titanium-based composite material EBSD test sample according to claim 1, characterized in that: In step S01, the step of mechanically polishing the sample includes: S011. Use sandpaper of different mesh sizes to polish the test surface until there are no obvious coarse scratches on the test surface and only fine scratches with the same direction can be observed; S012. Rough polishing of the test surface is performed using a chromium oxide polishing liquid, the mass fraction of the chromium oxide polishing liquid is 1-5%, the solvent is deionized water, the speed of the polishing machine is 200r / min-1000r / min, and the sample test surface is continuously cooled during the rough polishing process; S013. Use diamond polishing pastes of different specifications to polish the test surfaces respectively, and polish the test surfaces of the samples to a surface roughness Ra ≤ 0.8 μm.
3. The method for preparing a titanium-based composite material EBSD test sample according to claim 2, characterized in that: In step S011, the test surface is polished using sandpaper with gradually increasing mesh sizes, wherein the mesh size of the sandpaper is 120-2000 meshes.
4. The method for preparing a titanium-based composite material EBSD test sample according to claim 2, characterized in that: In step S012, the rotation speed of the grinding and polishing machine is 200r / min-600r / min.
5. The method for preparing a titanium-based composite material EBSD test sample according to claim 2, characterized in that: In step S013, the test surface is finely polished using diamond polishing paste with gradually increasing mesh sizes, and the specifications of the diamond polishing paste are W5.0-W1.
5.
6. The method for preparing a titanium-based composite material EBSD test sample according to claim 1, characterized in that: In step S02, the sample is immersed in anhydrous ethanol and ultrasonically cleaned for 5-15 minutes. After cleaning and drying the sample, the test surface is covered with an antistatic blue film.
7. The method for preparing a titanium-based composite material EBSD test specimen according to claim 1, characterized in that: In step S031, the voltage of the rough polishing treatment is 5 kV, the sample stage rotation angle is 10.5°, and the treatment time is 30 min; In step S032, the voltage of the fine polishing treatment is 4.5 kV, the rotation angle of the sample stage is 4.5°, and the treatment time is 45 minutes.
8. The method for preparing a titanium-based composite material EBSD test sample according to claim 1, characterized in that: When the test surface of the sample is subjected to triple ion beam polishing, the crack tip on the sample is located in the center of the sample stage.
9. The method for preparing a titanium-based composite material EBSD test sample according to claim 1, characterized in that: The sample is a titanium-based composite material including a titanium alloy matrix and a ceramic phase reinforcement.
10. The method for preparing a titanium-based composite material EBSD test specimen according to claim 1, characterized in that: The sample is a titanium-based composite material having an internal stress of 300-900 MPa after deformation or after a fatigue test.
Citation Information
Cited By
Measurement method of high-temperature alloy texture
CN119936088A
Preparation method of aluminum alloy sample containing silicon-rich particles for post-irradiation microscopic characterization
CN121678319A