Method for evaluating service life of thermoplastic polypropylene-based insulating material

By measuring volume resistivity and oxidation induction time, the Alenius equation is used to evaluate the life of thermoplastic polypropylene-based insulating materials, solving the problem of inefficient life evaluation in the prior art, and achieving rapid and economical life evaluation and state monitor.

CN118980900APending Publication Date: 2024-11-19SHANGHAI ELECTRIC CABLE RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411284441.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The prior art lacks a fast and efficient method for evaluating the lifetime and in-service state of thermoplastic polypropylene-based insulating materials, resulting in inefficient material aging process and consuming a lot of time and cost.

Method used

By measuring the volume resistivity and oxidation induction time at different temperatures, using the relationship between conductance activation energy and oxidation reaction activation energy, combined with the Arenius equation, a life evaluation equation is derived to achieve the expected life of thermoplastic polypropylene-based insulating materials. and rapid assessment of remaining life.

Benefits of technology

The rapid and efficient life evaluation of thermoplastic polypropylene-based insulating materials is achieved, which reduces time and economic costs, and can easily track material status, which is suitable for life monitoring of newly developed and in-service materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118980900A_ABST
    Figure CN118980900A_ABST
Patent Text Reader

Abstract

The invention relates to a service life evaluation method of a thermoplastic polypropylene-based insulating material, which comprises the following steps: measuring the volume resistivity of a newly developed thermoplastic polypropylene insulating material at different temperatures, and carrying out linear fitting to obtain conductive activation energy; and measuring the oxidation induction time of the thermoplastic polypropylene-based insulating material at different temperatures, associating the obtained conductive activation energy with the oxidation reaction activation energy according to a life equation based on the failure of the oxidation resistance of the material, and determining the expected life of the novel polypropylene-based thermoplastic insulating material. Measuring to obtain the initial oxidation induction temperature of the newly developed thermoplastic polypropylene-based insulating material and the oxidation induction temperature during failure; measuring corresponding oxidation induction temperatures of the thermoplastic polypropylene-based insulating material in different service times, and deducing an equation of residual life according to a life equation of the oxidation induction temperatures; and evaluating to obtain the residual life of the thermoplastic polypropylene-based insulating material under the service condition.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of insulating material diagnosis, and in particular relates to a life assessment method for thermoplastic polypropylene-based insulating materials. Background Art

[0002] Thermoplastic polypropylene-based insulation material is an insulation material based on polypropylene (PP). Polypropylene is a thermoplastic plastic with excellent chemical stability and electrical insulation properties.

[0003] At present, thermoplastic polypropylene insulation materials have become the preferred choice for replacing XLPE insulation in the power cable industry because they can meet the application requirements of 90°C without cross-linking, and have the characteristics of low environmental load and easy recycling after retirement; however, polypropylene-based materials are susceptible to heat and oxygen aging due to the methyl group (-CH3) at the tertiary carbon position of the molecular structure. Therefore, in the development process of thermoplastic polypropylene-based insulation materials, the oxidation resistance of polypropylene-based insulation materials is an important performance research indicator. As the main aging mode of organic insulation materials, the expected life of newly developed thermoplastic polypropylene insulation materials has always been the focus of attention in the application field.

[0004] Although the IEC60216 standard recommends the use of oven aging at different temperatures, and the test material elongation at break of 50% as the end of life extension evaluation of the thermal life of the material at the use temperature is widely used, but the material is aged in the oven at different temperature points, and IEC60216 requires that the aging time at the lowest test temperature is not less than 5000 hours, which means that it not only consumes a lot of time costs but also has low efficiency. In addition, the basis for determining that the elongation at break of the material is reduced by 50% is often inconsistent with the actual performance requirements of the insulation material;

[0005] Domestic and foreign researchers have conducted a lot of exploration and research on the life assessment methods of materials, striving to be close to the application performance requirements, and exploring from the ways to obtain activation energy and the determination of end of life. Taking XLPE insulation as an example, combined with the electrical performance requirements of the material, currently there are more multi-factor aging and performance test evaluations such as breakdown voltage-time, partial discharge-voltage withstand-thermal aging, etc. Attempts to introduce thermal analysis technology to quickly evaluate the life of materials have also been ongoing. The thermal decomposition temperature of the material at different heating rates is tested by TGA, and then the decomposition activation energy of the material is obtained by fitting the Arrhenius equation, and then the corresponding life equation is associated for rapid evaluation of the material. However, the aging of materials in actual application is a slow process, which undergoes a series of aging behaviors such as oxidation, volatilization of additives, and material molecular chain scission. Before the material decomposes, its related properties may fail.

[0006] Only by quickly and efficiently evaluating the life of thermoplastic polypropylene-based insulating materials can this type of material be promoted and applied; continuous tracking of the material's antioxidant properties after service and evaluating the status and remaining life of polypropylene-based insulating materials are also necessary operational diagnostic methods for the application of this material. However, the existing technology currently lacks a fast and efficient method for life assessment and in-service status diagnosis of this type of insulating material. Summary of the invention

[0007] The purpose of the present invention is to provide a life assessment method for thermoplastic polypropylene-based insulating materials, which can quickly and efficiently assess the expected life of thermoplastic polypropylene-based insulating materials, the state of the materials after operation, and the remaining life. In addition, the economic and time costs are low. To this end, the present application provides a life assessment method for thermoplastic polypropylene-based insulating materials, comprising the following steps:

[0008] Step 1: Measure the volume resistivity ρ of thermoplastic polypropylene-based insulation materials at different temperatures v (T), based on the temperature equation for volume resistivity:

[0009]

[0010] Transformation gives the equation:

[0011]

[0012] in:

[0013] ρ v (T) is the volume resistivity in ohm·meter (Ω·m);

[0014] A is the proportionality constant;

[0015] E c The conductivity activation energy is expressed in joules per mole (J / mol). The conductivity activation energy refers to the minimum energy required for electrons or ions to overcome potential barriers during the conduction process in the material. It indicates that in the conduction process, electrons or ions need to obtain sufficient energy to overcome scattering or obstacles in the material, thereby promoting the movement of charge carriers. As the temperature increases, the molecular motion of polypropylene insulation materials intensifies, the activity of carriers inside the material, such as free electrons or ions, increases, and the insulation resistivity of the material decreases.

[0016] R is the gas constant, which is 8.314 J / mol·K. The gas constant is a constant in the ideal gas state equation that relates the pressure, volume, and temperature of a gas. The gas constant R is the Boltzmann constant k B and Avogadro's constant N A The product of is as follows:

[0017] R = kB ×N A

[0018] Among them, N A is Avogadro's constant (N A ≈6.022×10 23 mol -1 ), which is the number of particles contained in each mole of a substance;

[0019] Boltzmann constant k B It is a basic constant in statistical mechanics, which connects the relationship between the energy and temperature of microscopic particles, such as molecules and atoms, and describes the relationship between the energy scale and temperature of a single particle;

[0020] Therefore, the gas constant R can also be converted by substituting the Boltzmann constant and Avogadro constant;

[0021] T is the test temperature, and the absolute temperature is taken in the calculation, with Kelvin as the unit, K;

[0022] It should be noted that the units in the formula can be converted to unified units according to measurement or calculation needs;

[0023] According to different temperatures The relationship between E and c ;

[0024] Step 2: For the newly developed thermoplastic polypropylene-based insulation material, the DSC technology was used to measure the oxidation induction time (OITP) of the material samples at different temperatures. t );

[0025] The Arrhenius equation is an empirical formula that describes the relationship between the chemical reaction rate constant and temperature. In chemical kinetics, it is used to explain how the chemical reaction rate changes with temperature.

[0026] According to the Arrhenius equation, the following equation for oxidation induction time is obtained:

[0027]

[0028] in:

[0029] A0 is the proportional constant;

[0030] E o The activation energy of oxidation reaction, measured in joules per mole (J / mol) or electron volts (eV). The activation energy of oxidation reaction refers to the minimum energy barrier that the reactants must overcome when the oxidation reaction occurs. Only when the reactant molecules obtain enough energy to reach the activated state can the oxidation reaction occur and continue.

[0031] R is the gas constant, which is 8.314 J / (mol·K). As in step 1, the gas constant R can also be converted by using the Boltzmann constant and Avogadro constant;

[0032] T is the temperature of the isothermal test condition, and the absolute temperature is taken in the calculation, with Kelvin as the unit, K;

[0033] τ is the oxidation induction time OITP t , life at temperature T, that is, failure time at temperature T;

[0034] The failure oxidation induction time at temperature T is regarded as the expected life of the material;

[0035] Oxidation Induction Time (OITP t Oxidation refers to the time before a material begins to oxidize significantly under specific conditions (such as high temperature and oxygen environment), which is used to evaluate the material's antioxidant properties; the type and content of antioxidants directly affect the material's oxidation induction time, and the appropriate amount of antioxidants can prolong the oxidation induction time;

[0036] Oxidation induction time test: The material sample is exposed to oxygen or air at a certain temperature, and the equipment determines the start time of the oxidation reaction by detecting the change in the heat flow of the sample; in the isothermal test process, the oxidation induction time is the time from when the material is switched from the protective nitrogen atmosphere to the oxygen atmosphere at the temperature to when the oxidation reaction occurs obviously;

[0037] Based on the failure of antioxidant performance, the activation energy E obtained in step 1 is c E o Associate, take E o =E c , OITP under isothermal conditions t To determine the expected life of thermoplastic polypropylene based insulation materials at service temperature;

[0038] The oxidation induction time OITP obtained so far t , i.e. the life at temperature T, is used to estimate the life of thermoplastic polypropylene-based insulation materials.

[0039] The present application provides a technical solution for a method for evaluating the life of a thermoplastic polypropylene-based insulating material, which also includes the following technical features:

[0040] Preferably, in one embodiment of the present application, in step 3, the initial oxidation induction temperature (OITP) of the newly developed thermoplastic polypropylene-based insulating material is obtained. i ) and the oxidation induction temperature at failure (OITP k ), based on existing data or using DSC technology to measure activities;

[0041] The oxidation induction temperature refers to the temperature at which a material begins to undergo a significant oxidation reaction under specific test conditions (usually at a constant heating rate); that is, when the material is heated in an oxygen environment, the material begins to oxidize rapidly after reaching this temperature.

[0042] The initial oxidation induction temperature refers to the oxidation induction temperature of the material before it undergoes any oxidation degradation; it reflects the antioxidant capacity of the material in its initial state; that is, the temperature obtained by directly testing the oxidation induction temperature of the material without aging or use is the initial oxidation induction temperature, which reflects the antioxidant capacity of the newly developed insulating material in its initial state;

[0043] The oxidation induction temperature at failure refers to the failure of the material's antioxidant properties after use or aging. The value obtained when measuring its oxidation induction temperature is close to that of pure resin without antioxidants.

[0044] Step 4: Measure different service times t m The corresponding oxidation induction temperature (OITP) of thermoplastic polypropylene-based insulation materials m ), according to OITP m The functional relationship equation is:

[0045]

[0046] get

[0047]

[0048] OITP of material failure under the same conditions K The corresponding function should be:

[0049]

[0050] Organize first

[0051]

[0052] Substitution

[0053]

[0054] get

[0055]

[0056] Introduce the remaining life (t s ) equation:

[0057]

[0058] t sfor the remaining life;

[0059] t m For service time;

[0060] Obtain the remaining life t of thermoplastic polypropylene-based insulation materials under service conditions s , which allows for quick and easy life assessment and tracking of material status.

[0061] Preferably, in one embodiment of the present application, in step 1, the volume resistivity of the thermoplastic polypropylene insulating material is tested with reference to GB / T31838.2.

[0062] Preferably, in one embodiment of the present application, in step one, the test temperature T of the volume resistivity of the thermoplastic polypropylene-based insulating material is between the glass transition point temperature Tg and the melting point temperature Tm of the material; the glass transition temperature refers to the temperature at which an amorphous or semi-crystalline polymer material changes from a glass state to a rubber state.

[0063] Preferably, in one embodiment of the present application, in step 1, the measured temperature T is: Tg-20°C≦T≦Tm-20°C.

[0064] Preferably, in one embodiment of the present application, in step 1, 30°C≦T≦130°C.

[0065] Preferably, in one embodiment of the present application, in step 1, The fitting factor is not less than 99%.

[0066] Preferably, in one embodiment of the present application, in step 2, the oxidation induction time OITP t Refer to GB / 19466.6 for implementation.

[0067] Preferably, in one embodiment of the present application, in step 2, the sample size of the flake sample is 6 mg-10 mg , parallel comparison sample amount deviation ≤ 0.5 mg, isothermal conditions, O2 atmosphere, gas flow 50 ml / min ~ 100 ml / min;

[0068] Determine the life of thermoplastic polypropylene-based insulation materials, select the oxidation induction time OITP under isothermal test conditions t The expected lifespan is evaluated by correlating the numerical results with the range of 30 minutes ≦ oxidation induction time (OITP). t ≦60 minutes.

[0069] Preferably, in one embodiment of the present application, in step 3, the DSC test sampling requirements are: sheet sample, 8 mg ± 0.5 mg; heating rate is not greater than 10 ° C / min, based on GB / 19466.6 test thermoplastic polypropylene-based insulating material initial oxidation induction temperature OITP i and the oxidation induction temperature (OITP) at failure k ;

[0070] DSC test refers to Differential Scanning Calorimetry test, which is a thermal analysis technique used to study the thermal properties of materials. DSC test can measure the temperature-related energy changes of materials during heating or cooling. These energy changes are related to physical or chemical changes of materials.

[0071] Preferably, in one embodiment of the present application, in step 3, the initial oxidation induction temperature OITP i OITP is the initial oxidation induction temperature of the newly developed thermoplastic polypropylene insulation material and the oxidation induction temperature at failure k is the oxidation induction temperature of pure polypropylene matrix resin; the average value is obtained by measuring three times;

[0072] The newly developed thermoplastic polypropylene insulation material, that is, the target object of the life evaluation, that is, the material to be evaluated in this application, is tested according to the newly developed thermoplastic polypropylene insulation material, and the oxidation induced temperature (OITP) at failure is k , directly using pure polypropylene matrix resin oxidation induction temperature;

[0073] Pure polypropylene matrix resin is the PP matrix raw material of thermoplastic polypropylene insulation material;

[0074] Pure resin cannot be used without adding additives, so the oxidation induction temperature of the modified thermoplastic polypropylene insulation material at failure is the oxidation induction temperature value of the pure polypropylene matrix resin.

[0075] Preferably, in one embodiment of the present application, in step 4, the service time t m Thermoplastic polypropylene-based insulation materials under the condition of in-service sampling test, sheet specimens, sample size 8mg±0.5mg, heating rate not more than 10℃ / min, based on GB / 19466.6 test thermoplastic polypropylene-based insulation material oxidation induction temperature OITP m , measure three times and take the average value.

[0076] Preferably, in one embodiment of the present application, in step 4, the oxidation induction temperature OITP is measured. m, combined with the initial oxidation induction temperature OITP obtained in step 3 i and the oxidation induction temperature (OITP) at failure k Value, determine the remaining life t of thermoplastic polypropylene insulation material in service s The unit of oxidation induction temperature is K, and the unit of remaining life is year (y), or it can be converted into day, hour or minute.

[0077] The beneficial effects of this application are:

[0078] 1. The present application provides a life assessment method for thermoplastic polypropylene-based insulating materials, which can achieve rapid and efficient assessment of the expected life of thermoplastic polypropylene-based insulating materials, as well as the state and remaining life of the materials after operation; and the economic and time costs are low;

[0079] 2. The present application provides a life verification method for thermoplastic polypropylene-based insulating materials, which is used to calculate the remaining life of thermoplastic polypropylene-based insulating materials under service conditions, especially the remaining life after a period of service, for monitoring the operating status; in nuclear power and some special application occasions, such as when it is impossible to extract samples for actual measurement; using the technical solution of the present application, it is very convenient to conduct remaining life evaluation;

[0080] 3. This application reduces the testing cost in calculating the remaining life assessment after a period of service by using the initial oxidation induction temperature OITP i OITP is the initial oxidation induction temperature of the newly developed thermoplastic polypropylene insulation material and the oxidation induction temperature at failure k The oxidation induction temperature of pure polypropylene matrix resin can be directly used to quickly evaluate and track the material status, thus reducing the cost of evaluation and testing;

[0081] 4. This application provides a life assessment method for thermoplastic polypropylene-based insulating materials, providing design and application engineering data reference for the practical application of thermoplastic polypropylene-based insulating materials, namely how to isolate the structural design protection of oxygen, and the status tracking and diagnosis after service. BRIEF DESCRIPTION OF THE DRAWINGS

[0082] Figure 1 A flow chart of the steps of a method for evaluating the life of a thermoplastic polypropylene-based insulating material of the present invention;

[0083] Figure 2 The method for evaluating the life of a thermoplastic polypropylene-based insulating material according to the present invention is as follows: Relationship diagram;

[0084] Figure 3The isothermal 190°C OITP of step 2 of the life evaluation method of a thermoplastic polypropylene-based insulating material of the present invention is t Measurement graphs;

[0085] Figure 4 The isothermal OITP at 200°C of step 2 of the life evaluation method of thermoplastic polypropylene-based insulation material of the present invention is t Measurement graphs;

[0086] Figure 5 The isothermal OITP at 210°C of step 2 of the life evaluation method of a thermoplastic polypropylene-based insulating material of the present invention is t Measurement graphs;

[0087] Figure 6 The isothermal OITP at 220°C of step 2 of the life evaluation method of thermoplastic polypropylene-based insulation material of the present invention is t Measurement graphs;

[0088] Figure 7 The initial thermal decomposition temperature OITP of the thermoplastic polypropylene insulating material in step 3 of the life evaluation method of the thermoplastic polypropylene-based insulating material of the present invention is i Measurement graphs;

[0089] Figure 8 It is a graph showing the oxidation induced temperature measurement of a PP-based raw material in a method for evaluating the life of a thermoplastic polypropylene-based insulating material according to the present invention;

[0090] Fig. 9 is the oxidation induction temperature OITP of the thermoplastic polypropylene insulating material after service in step 4 of the method for evaluating the life of a thermoplastic polypropylene-based insulating material of the present invention. m Measurement curve graph. DETAILED DESCRIPTION

[0091] The specific implementation methods of the present application are further described in detail below in conjunction with the accompanying drawings. These implementation methods are only used to illustrate the present application, and are not intended to limit the present invention.

[0092] In the description of the present invention, it should be noted that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are used for descriptive purposes only and cannot be understood as indicating or implying relative importance.

[0093] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0094] Furthermore, in the description of the present invention, unless otherwise specified, “plurality” means two or more.

[0095] like Figure 1 , a life evaluation method for thermoplastic polypropylene-based insulating materials, comprising the following steps:

[0096] Step 1: Refer to GB / T31838.2 to test the volume resistivity ρ of thermoplastic polypropylene (PP) insulation material at 50℃, 70℃, 90℃, and 110℃ respectively v (T), the test results are shown in Table 1.

[0097] Table 1 Volume resistivity of polypropylene-based insulation materials at different temperatures

[0098]

[0099] First convert the temperature to uniform units:

[0100]

[0101] According to the data in Table 1, based on the temperature equation of volume resistivity:

[0102]

[0103] Sure Relationship, linear fitting see attached Figure 2 , the fitting degree is 99.9%, given by Figure 2 You will get:

[0104] lnA≈-5.91947

[0105]

[0106] R=8.314J / (mol·K)

[0107] Calculation results:

[0108] E c ≈105250 J / mol

[0109] For thermoplastic polypropylene insulation material, the conductivity activation energy E obtained by linear fitting in step 1 is c The fitting degree is very high, which well reflects the temperature dependence of the volume resistivity of the insulating material.

[0110] The obtained electrical conductivity activation energy reflects the activation energy of the conductive carriers inside the material, which is related to the oxidation resistance of the thermoplastic polypropylene insulation material to a certain extent.

[0111] Specifically, in one embodiment of the present application, in step 2, the oxidation induction time of the thermoplastic polypropylene-based insulating material is measured by using the DSC technology according to GB / 19466.6. The test curve is shown in the attached Figure 3-6 ;

[0112] Take the OITP at 200℃ t The value of 53.43min is used as a reference to calculate the expected life of thermoplastic polypropylene-based insulation materials at the maximum operating temperature of 90°C required for power cables; according to the oxidation induction time (OITP t ) satisfies the Arrhenius equation:

[0113]

[0114] Then we have:

[0115]

[0116] Substitute E o Value

[0117] E o =E c

[0118]

[0119]

[0120]

[0121] τ 200℃=53.43min

[0122] get:

[0123] τ 90℃ =176767.818min

[0124] It is further calculated that at an operating temperature of 90°C and exposed to an oxygen atmosphere, the expected life of the insulating material based on the failure of its oxidation resistance is 122 days.

[0125] Specifically, in one embodiment of the present application, in step 3, the DSC technology is used with reference to GB / 19466.6, such as Figure 7 , 8 ,according to Figure 8 It is the oxidation induced temperature measurement curve of PP-based raw materials. Therefore, the oxidation induced temperature OITP at failure is taken k is 217.31℃;

[0126] Measuring the Oxidation Induction Temperature (OITP) of Thermoplastic Polypropylene Insulation Materials i and the initial oxidation induction temperature of pure polypropylene resin to obtain the initial oxidation induction temperature OITP of thermoplastic polypropylene insulation material i = 257.19°C, and the oxidation induction temperature (OITP) at which thermoplastic polypropylene insulation fails k =217.31℃,

[0127] Step 3: Use DSC technology to refer to GB / 19466.6 to measure the service time t of thermoplastic polypropylene insulation material m Oxidation Induction Temperature (OITP) m , see attached Fig. 9 , OITP m =240.37℃,t m = 10 years;

[0128] Step 4: Based on OITP i =257.19℃, OITP k =217.31℃ and OITP tested under service conditions m =240.37℃, based on oxidation induction temperature OITP m Remaining life (t s ) equation:

[0129] Convert the given temperature value to Kelvin:

[0130] OITP i =257.19+273.15=530.34K

[0131] OITP k=217.31+273.15=490.46K

[0132] OITP m =240.37+273.15=513.52K

[0133] Substitution

[0134]

[0135] t s =1.482t m

[0136] The remaining life of the insulating material under service conditions can be evaluated based on the loss of oxidation resistance. s It is 14.82 years.

[0137] In summary, the present invention aims to solve the existing life assessment method of thermoplastic polypropylene-based insulating materials, including adopting a step-by-step temperature increase method to measure the volume resistivity of thermoplastic polypropylene-based insulating materials at different temperatures, and obtaining the conductivity activation energy of the insulating material by fitting; measuring the oxidation induction time of thermoplastic polypropylene-based insulating materials at different temperatures; correlating the conductivity activation energy with a life equation based on the failure of the material's antioxidant performance, and quickly evaluating the life of the thermoplastic polypropylene-based insulating material; measuring the initial oxidation induction temperature of the thermoplastic polypropylene-based insulating material, the oxidation induction temperature at the end of the life, and correlating with the oxidation induction temperature of the material sample after service to infer the remaining life of the material after service; the inventive method can not only predict the life of the newly developed thermoplastic polypropylene-based insulating material, but also perform quality control on the remaining life of the material after service; the inventive method is also suitable for the life assessment of organic insulating materials with high antioxidant performance requirements, and has the characteristics of being simple, efficient and quick to evaluate.

[0138] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and substitutions can be made without departing from the technical principles of the present invention. These improvements and substitutions should also be regarded as the scope of protection of the present invention.

Claims

1. A method for evaluating the life of a thermoplastic polypropylene-based insulating material, characterized in that: The steps include: Step 1: Measure the volume resistivity of thermoplastic polypropylene-based insulation materials at different temperatures, based on the temperature equation of volume resistivity: Transformation gives the equation: in: ρ v (T) is volume resistivity; A is the proportionality constant; E c is the conductivity activation energy; R is the gas constant; T is the test temperature; According to different temperatures The relationship between E and c ; Step 2: Measure the oxidation induction time (OITP) of thermoplastic polypropylene-based insulation materials at different temperatures t , based on the life equation of the material's anti-oxidation performance failure: in: A0 is the proportional constant; E o is the activation energy of the oxidation reaction, and E o =E c ; R is the gas constant; T is the temperature of the isothermal test condition; τ is the oxidation induction time OITP t , lifespan at temperature T.

2. A method for evaluating the life of a thermoplastic polypropylene-based insulating material according to claim 1, characterized in that: In step 1, the test temperature T of the volume resistivity of the thermoplastic polypropylene-based insulating material is between the glass transition point temperature Tg and the melting point temperature Tm of the material.

3. A method for evaluating the life of a thermoplastic polypropylene-based insulating material according to claim 1, characterized in that: Step 3: Obtaining the initial oxidation induction temperature OITP of thermoplastic polypropylene-based insulation material i and the oxidation induction temperature (OITP) at failure k ; Step 4: After the thermoplastic polypropylene-based insulation material has been put into service, measure the different service times t m The corresponding oxidation induction temperature (OITP) of thermoplastic polypropylene-based insulation materials m , according to the oxidation induction temperature OITP m The functional relationship equation is: Under the same conditions, thermoplastic polypropylene-based insulation material OITP K The equation is: Get the remaining life t s The equation is: Obtain the remaining life t of thermoplastic polypropylene-based insulation materials under service conditions s , track the status of materials.

4. A method for evaluating the life of a thermoplastic polypropylene-based insulating material according to claim 1, characterized in that: In step 2, the life of thermoplastic polypropylene-based insulation materials is determined by selecting the oxidation induction time (OITP) under isothermal test conditions. t The expected lifespan is evaluated by correlating some numerical results. The range of some numerical results is: 30 minutes ≦ oxidation induction time OITP t ≦60 minutes.

5. A method for evaluating the life of a thermoplastic polypropylene-based insulating material according to claim 3, characterized in that: In step 3, a DSC test is performed to obtain the initial oxidation induction temperature OITP of the thermoplastic polypropylene-based insulating material. i and the oxidation induction temperature (OITP) at failure k .

6. A method for evaluating the life of a thermoplastic polypropylene-based insulating material according to claim 3, characterized in that: In step 3, the initial oxidation induction temperature OITP i OITP is the initial oxidation induction temperature of the newly developed thermoplastic polypropylene insulation material and the oxidation induction temperature at failure k OITP is the oxidation induction temperature of polypropylene matrix resin at failure k .

7. A method for evaluating the life of a thermoplastic polypropylene-based insulating material according to claim 3, characterized in that: In step 4, the service time t m Thermoplastic polypropylene based insulation materials under in-service conditions are sampled and tested to test the oxidation induced temperature (OITP) of thermoplastic polypropylene based insulation materials. m .

8. A method for evaluating the life of a thermoplastic polypropylene-based insulating material according to claim 3, characterized in that: In step 4, the oxidation induction temperature OITP is measured. m According to step 3, the initial oxidation induction temperature OITP is obtained i and the oxidation induction temperature (OITP) at failure k Value, determine the remaining life t of thermoplastic polypropylene insulation material in service s .

9. A method for evaluating the life of a thermoplastic polypropylene-based insulating material according to claim 1, characterized in that: In step 1, the measurement temperature T is: Tg-20°C≦T≦Tm-20°C.

10. A method for evaluating the life of a thermoplastic polypropylene-based insulating material according to claim 2, characterized in that: In step 1, the measurement temperature T is preferably: 30°C ≦ T ≦ 130°C; The fitting factor is not less than 99%.