Variable-temperature self-adaptive elastic concrete, composite structure and related design method
Through adaptive elastic concrete design of temperature variable temperature and finite element analysis, a temperature stress and fatigue damage model was established, which solved the cracking problem of concrete composite structures under large temperature difference environment, and achieved a design of high crack resistance and rational utilization of resources.
Patent Information
- Application Number
- CN202411047812.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
AI Technical Summary
The existing concrete composite structure design methods lack theoretical basis and repeatability in a large temperature difference environment, which cannot effectively prevent the cracking problem of concrete structures, and insufficient crack resistance improvement measures.
Adaptive elastic concrete design method of temperature variable temperature, combined with finite element analysis technology, a temperature stress transmission model and a temperature fatigue accumulation damage model are established, and the cracked parts and maximum depth of the concrete structure are determined, and the 'inner rigid and externally extended' type high-crack-resistant elastic concrete composite is designed. Structure: The low-temperature high-mode-high-temperature low-mode characteristics of the material are achieved through polyurethane modified materials.
It significantly improves the crack resistance and adaptability of concrete structures under large temperature differences, increases the ultimate strain rate by 180% to 250%, and increases the elastic energy absorption effect by 100% to 240%, avoids plastic cracking, and realizes the rationality of resources. use.
Smart Images

Figure CN118983033A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of concrete materials and structures, and more particularly to a temperature-adaptive elastic concrete, a composite structure and a related design method. Background Art
[0002] At present, structural cracking under the action of temperature cycles has become a major challenge faced by concrete structures during their service in areas with large temperature differences. In order to solve the problem of cracking of concrete structures in areas with large temperature differences, existing studies often use fiber toughening technology to improve the crack resistance of concrete, and design composite structures to reduce the cost of use, so that each part of the structure can "perform its own function". The patent "An intelligent FRP-concrete composite structure and its manufacturing method (CN201210380940.9)" invented an intelligent fiber-reinforced resin composite material based on carbon fiber distributed sensing, proposed a method for manufacturing an intelligent FRP-concrete composite structure, and realized real-time monitoring of structural service data by using the conductive properties of carbon fiber. The patent "Hybrid Fiber Reinforced Resin Composite Concrete Composite Structure and Its Manufacturing Method (CN200610037891.3)" invented a hybrid fiber reinforced resin composite concrete and composite structure preparation method. The composite structure is a rectangular cross-section composite structure composed of a hybrid FRP outer coating layer and a cast-in-place concrete core, which effectively controls the cracking of the concrete structure. However, the composite structure does not specify the design method of the inner and outer layer dimensions of the composite structure, and still cannot achieve the reasonable use of new anti-cracking concrete materials and traditional concrete materials. The patent "Steel Fiber Polymer Concrete Composite Structure and Its Preparation Method and Application (CN201610077878.4)" invented a steel fiber polymer concrete, and proposed a composite structure design method for bending members in a targeted manner according to the main bending parts of the bending members. The composite structure prepared in this way has the advantages of high strength, high toughness, and good deformation coordination. However, this method is mainly aimed at improving the bending strength and toughness of concrete under bending loads, and has no obvious effect on the crack resistance of the concrete surface under temperature fatigue stress.
[0003] The current concrete composite structure design methods still have the following problems:
[0004] (1) At present, composite structures mainly use the bridging effect of fibers to enhance the bending bearing capacity and toughness of bending structures such as bridges. However, there is little research on the cracking mechanism and measures to improve the crack resistance of concrete structures in large temperature difference environments.
[0005] (2) Composite structural concrete enables each part of the concrete structure to "perform its own function", but existing research mostly involves forming a large number of composite structures with different proportions and comparing them to find the "optimal proportion". This lacks theoretical basis and has poor repeatability. A theoretical design basis and design method for concrete composite structures have not yet been proposed, and it is impossible to form a design system for crack-resistant concrete composite structures for actual large temperature difference environments.
[0006] Therefore, how to construct a concrete composite structure design system and realize repeatable design of concrete composite structures under large temperature difference environments is an urgent problem to be solved by technical personnel in this field. Summary of the invention
[0007] In view of this, the present invention provides a variable temperature adaptive elastic concrete, a composite structure and a related design method. The independently developed variable temperature adaptive elastic concrete has the unique property of "low temperature high modulus - high temperature low modulus" that the modulus can be controlled with temperature, which can effectively prevent the cracking problem of the concrete structure under the action of temperature fatigue stress. At the same time, in order to reasonably use the variable temperature adaptive elastic concrete material, a temperature stress transfer model and a temperature fatigue cumulative damage model of the concrete structure in a large temperature difference environment are proposed, and the cracking of the sunny side and the shady side of the concrete structure in a large temperature difference environment are simulated based on the finite element analysis technology. The location, maximum depth and damage development law of the cracking of the concrete structure in a large temperature difference environment are clarified, and a design method for the "inner rigid and outer extension" type high crack resistance elastic concrete composite structure column with polyurethane modified concrete outer coating for crack resistance and conventional concrete inner casting for bearing is proposed. While ensuring that the concrete structure has high resistance to temperature fatigue cracking, it achieves the rational use of resources and realizes the parameter matching design system of high crack resistance concrete composite structure based on the actual large temperature difference environment.
[0008] In order to achieve the above object, the present invention adopts the following technical solution:
[0009] A method for designing temperature-adaptive elastic concrete, wherein the content of each component of the temperature-adaptive elastic concrete is determined as follows:
[0010] Step 11: Collect ambient temperature difference data;
[0011] Step 12: Obtain the actual size of the concrete structure, conventional concrete pouring mix ratio and basic mechanical performance indicators of the concrete structure;
[0012] Step 13: According to the actual size of the concrete structure, the conventional concrete pouring mix ratio and the basic mechanical performance index of the concrete structure, a concrete structure model is constructed using a finite element analysis system, and a temperature deformation model is obtained by combining a temperature stress transfer model and a temperature fatigue cumulative damage model; the ambient temperature difference data is input into the temperature deformation model to obtain the cracking location, maximum cracking depth and initial cracking time of the concrete structure model;
[0013] Step 14: Determine the mix ratio of the temperature-adaptive elastic concrete according to the mapping relationship between the mix ratio of the temperature-adaptive concrete and the first crack time.
[0014] Preferably, the basic principle of the temperature stress transfer model is: obtaining the corresponding local temperature difference of concrete under the ambient temperature difference according to the ambient temperature difference data and the concrete structure model; in a large temperature difference environment, the concrete generates a temperature gradient under the action of the ambient temperature difference and the local temperature difference of the concrete, and the contraction and expansion of the concrete structure are restricted during the temperature gradient change process, thereby generating self-constrained temperature stress and surface temperature stress, as shown below:
[0015]
[0016] Where a is the linear expansion coefficient of concrete (℃-1); ΔT 1 (t) is the temperature difference between the center and the surface of the concrete obtained according to the ambient temperature difference data and the concrete structure model (°C); K(t,τ) is the stress relaxation coefficient of the concrete; E(t) represents the elastic modulus of the concrete; t is the stress generation time (s); τ is the stress retention time (s); ΔT 2 (t) is the reduction of the comprehensive temperature difference of concrete obtained according to the ambient temperature difference data and the concrete structure model; R(t) is the generalized constraint coefficient; C X is the external constraint horizontal deformation stiffness (N·m -3 ), H is the thickness of the concrete structure (m), and L is the length of the concrete structure (m).
[0017] Preferably, the basic principle of the temperature fatigue cumulative damage model is: the local temperature difference of the concrete corresponding to the ambient temperature difference is obtained according to the ambient temperature difference data and the concrete structure model; the temperature stress generated by the temperature gradient inside and outside the concrete structure under the action of the day and night temperature cycle increases and decreases periodically, and the temperature fatigue stress causes the internal damage of the concrete structure to gradually accumulate until a certain limit is reached, causing the concrete structure to crack.
[0018] Preferably, the damage variable Dc calculated by the thermal fatigue cumulative damage model is expressed as:
[0019]
[0020] Where, dD c is the increment of fatigue damage; du m is the deformation increment; u m is the deformation; u ε is the cumulative deformation under temperature fatigue; T is the current stress increment; ft is the initial maximum normal stress; δ 0 is the deformation threshold; Cf is the correction factor (0 <Cf<1)。
[0021] Preferably, if cracking occurs in a concrete structure under thermal fatigue stress, the following criteria should be met simultaneously:
[0022] Failure occurs only when the strain exceeds the ultimate tensile strain of concrete;
[0023] The extent of damage increase depends on the change of concrete strain. Concrete cracking will occur only when the damage variable reaches a certain threshold.
[0024] Preferably, for C40-C80 concrete, the damage variable threshold for concrete cracking is that the concrete will not crack until the damage variable reaches 0.2-0.3.
[0025] Preferably, the strain limit value at which concrete will not be damaged under the action of temperature fatigue is, for C40-C80 concrete, 0.2-0.4 times the ultimate tensile strain of the concrete material.
[0026] A method for designing a temperature-adaptive elastic concrete composite structure comprises the following steps:
[0027] Step 21: Clarify the meteorological data of the environment where the concrete structure is located, obtain the monthly average day and night temperature difference of the area, and obtain the environmental temperature difference data;
[0028] Step 22: Determine the actual size of the concrete composite structure, conventional concrete pouring mix ratio and basic mechanical performance indicators;
[0029] Step 23: The actual size of the concrete composite structure, the conventional concrete pouring mix ratio and the basic mechanical performance index of the concrete structure are imported into a finite element analysis system to construct a concrete structure model, and a temperature deformation model is obtained by combining a temperature stress transfer model and a temperature fatigue cumulative damage model; the ambient temperature difference data is input into the temperature deformation model to calculate the cracking position, maximum cracking depth and initial cracking time of the concrete structure model;
[0030] Step 24: determining the mix ratio of the temperature-adaptive elastic concrete according to the mapping relationship between the mix ratio of the temperature-adaptive concrete and the first crack time;
[0031] Step 25: Steps 21-23 are to carry out simulations for several years, with the maximum cracking depth of the concrete structure model within the service life as the dividing line. The proportion of variable temperature adaptive elastic concrete in the concrete composite structure is determined according to the dividing line, and a variable temperature adaptive elastic concrete composite structure is constructed. The outer layer of the dividing line is constructed with a variable temperature adaptive elastic concrete layer, and the inner layer is constructed with a conventional concrete layer. The design obtains an "inner rigid and outer extension" type variable temperature adaptive elastic concrete composite structure with variable temperature adaptive elastic concrete on the outer layer and conventional concrete on the inner layer.
[0032] Preferably, the maximum crack depth boundary line of the concrete structure within the service life is defined as a closed curve formed by connecting the positions where the internal damage variable of the concrete structure within the designed service life is 0.
[0033] A temperature-adaptive elastic concrete comprises cement, machine-made sand, 5mm-10mm graded crushed stone, 10mm-20mm graded crushed stone, group A waterborne polyurethane, group B waterborne polyurethane, water-reducing and defoaming functional components and water.
[0034] Preferably, the dosage of the raw material components of the temperature-adaptive elastic concrete is: cement 300kg / m 3 ~600kg / m 3 , Machine-made sand 400kg / m 3 ~800kg / m 3 , 5mm~10mm graded crushed stone 300kg / m 3 ~700kg / m 3 , 10mm~20mm graded crushed stone 400kg / m 3 ~800kg / m 3 、Group A waterborne polyurethane 10kg / m 3 ~50kg / m 3 、Group B waterborne polyurethane 5kg / m 3 ~25kg / m 3 , water-reducing and defoaming functional components 0kg / m 3 ~50kg / m 3 、Water 50kg / m 3 ~200kg / m 3 .
[0035] Preferably, the waterborne polyurethane of group A is mainly prepared from the following raw materials in parts by weight: 30 to 80 parts of macromolecular diol, 30 to 60 parts of hydrophilic chain extender, 1 to 10 parts of ethylene oxide, 1 to 5 parts of organic tin compound, and 1 to 5 parts of antioxidant; the waterborne polyurethane of group B is mainly prepared from the following raw materials in parts by weight: 60 to 90 parts of diisocyanate, 10 to 20 parts of organic amine compound and other raw materials.
[0036] The technical effect of the above technical scheme is that the ultimate strain rate of the variable temperature adaptive elastic concrete is increased by 180% to 250% compared with conventional concrete, the elastic energy absorption effect is increased by 100% to 240%, and the modulus of the variable temperature adaptive elastic concrete is controllable with temperature, and when the ambient temperature rises by 40°C, the elastic modulus of the variable temperature adaptive elastic concrete decreases by 15% to 25%. By reducing the elastic modulus, its deformation adaptability is improved, thereby avoiding plastic cracking of the concrete.
[0037] A variable temperature self-adaptive elastic concrete composite structure comprises an outer layer structure and an inner layer structure, wherein the outer layer structure adopts variable temperature self-adaptive elastic concrete.
[0038] Preferably, the inner layer structure adopts conventional concrete.
[0039] It can be seen from the above technical solutions that, compared with the prior art, the present invention discloses a variable temperature adaptive elastic concrete, a composite structure and a related design method, which have the following beneficial effects:
[0040] (1) The temperature-adaptive elastic concrete material developed based on waterborne polyurethane modification technology has the advantages of small strength change before and after modification, strong elastic energy absorption effect, high ultimate strain rate, small strength loss at high temperature, and good crack resistance under temperature fatigue stress. At the same time, the highly crack-resistant elastic concrete material also has the characteristics of "high modulus at low temperature-low modulus at high temperature" whose modulus can be controlled with temperature, which improves the adaptability of concrete structures in large temperature difference environments;
[0041] (2) A method for predicting the cracking of concrete structures in an actual large temperature difference environment was established: the concrete structure temperature stress transfer model and the temperature fatigue cumulative damage model were used to define the damage mechanism and cracking characteristics of concrete structures in a large temperature difference environment. The finite element analysis method was used to intuitively reflect the entire process from damage accumulation to cracking of concrete structures in a large temperature difference environment based on the actual large temperature difference environment conditions.
[0042] (3) A design method for a "rigid inside and extended outside" concrete composite structure that is suitable for a large temperature difference environment is proposed: Based on the finite element calculation results of the concrete structure under a large temperature difference environment, the damage and cracking of the concrete structure within the designed service life can be analyzed, and based on the closed curve composed of the parts where the internal damage variable of the concrete structure is 0 within the service life, the ratio of the external "high crack resistance" variable temperature adaptive elastic concrete and the internal "high load-bearing" conventional concrete is designed to achieve a high crack resistance concrete composite structure design that meets the actual large temperature difference environment characteristics. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0044] Figure 1 A schematic diagram of the process flow of the temperature-adaptive elastic concrete design method provided by the present invention;
[0045] Figure 2 A schematic diagram of the process flow of the temperature-adaptive elastic concrete composite structure design method provided by the present invention;
[0046] Figure 3 A schematic diagram of a simulation of a concrete composite structure in Example 5 provided by the present invention;
[0047] Figure 4 A schematic diagram of damage simulation of a concrete composite structure in Example 5 provided by the present invention;
[0048] Figure 5 A schematic diagram of a simulation of a concrete composite structure in Example 6 provided by the present invention;
[0049] Figure 6 A schematic diagram of damage simulation of a concrete composite structure in Example 6 provided by the present invention;
[0050] Figure 7 A schematic diagram of a simulation of a concrete composite structure in Example 7 provided by the present invention;
[0051] Figure 8 This is a schematic diagram of damage simulation of the concrete composite structure in Example 7 provided by the present invention. DETAILED DESCRIPTION
[0052] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0053] Example 1
[0054] The embodiment of the present invention discloses a method for designing temperature-adaptive elastic concrete, comprising the following steps:
[0055] S11: Determine the meteorological data of the environment where the concrete structure is located and obtain the monthly average day and night temperature difference of the area;
[0056] S12: Obtain the actual size of the concrete structure, conventional concrete pouring mix ratio and basic mechanical performance indicators of the concrete structure;
[0057] S13: Import the field parameters in S11 and S12 into the finite element analysis system, and use the independently developed temperature stress transfer model and temperature fatigue cumulative damage model to calculate the cracking location, maximum cracking depth and initial cracking time of the concrete structure;
[0058] S14: Determine the temperature-adaptive elastic concrete mix ratio according to the relationship between the preset temperature-adaptive concrete mix ratio and the first cracking time; the first cracking time is less than or equal to 1 year, 1 year to 2 years, 2 years to 5 years, and greater than 5 years, which correspond to different temperature-adaptive concrete mix ratios.
[0059] Furthermore, the basic principle of the temperature stress transfer model is that in a large temperature difference environment, concrete generates a temperature gradient under the action of the ambient temperature difference and the local temperature difference of the concrete. During the temperature gradient change process, the contraction and expansion of the concrete structure are restricted, thereby generating self-constrained temperature stress and surface temperature stress, as shown below:
[0060]
[0061] Where a is the linear expansion coefficient of concrete (℃-1); ΔT 1 (t) is the temperature difference between the center and surface of concrete obtained by simulating the concrete structure model according to the ambient temperature difference (℃); K(t,τ) is the stress relaxation coefficient of concrete; E(t) represents the elastic modulus of concrete; t is the stress generation time (s); τ is the stress retention time (s); ΔT 2 (t) is the reduction of the comprehensive temperature difference of concrete obtained by simulating the concrete structure model according to the ambient temperature difference; R(t) is the generalized constraint coefficient; C X is the external constraint horizontal deformation stiffness (N·m -3 ), H is the thickness of the concrete structure (m), and L is the length of the concrete structure (m).
[0062] Furthermore, the basic principle of the temperature fatigue cumulative damage model is that the temperature stress generated by the temperature gradient inside and outside the concrete structure under the action of the day and night temperature cycle increases and decreases periodically, and the temperature fatigue stress causes the internal damage of the concrete structure to gradually accumulate until it reaches a certain limit and causes the concrete structure to crack; the temperature fatigue cumulative damage model is expressed as the damage variable Dc:
[0063]
[0064] Where, dD c is the increment of fatigue damage; du m is the deformation increment; u mis the deformation; u ε is the cumulative deformation under temperature fatigue; T is the current stress increment; ft is the initial maximum normal stress; δ 0 is the deformation threshold; C f is the correction factor (0 <Cf<1)。
[0065] Furthermore, if cracking occurs in concrete structures under thermal fatigue stress, the following criteria should be met simultaneously:
[0066] Failure occurs only when the strain exceeds the ultimate tensile strain of concrete;
[0067] The degree of damage increase depends on the change of concrete strain. When the damage variable reaches a certain threshold, concrete will crack.
[0068] There is a certain limit value for the strain of concrete under temperature fatigue. Once the strain is lower than this limit value, the material will not suffer fatigue failure no matter how many times it cycles.
[0069] Furthermore, for C40-C80 concrete, the damage variable threshold for concrete cracking is that the concrete will only crack when the damage variable reaches 0.2-0.3.
[0070] Furthermore, the strain limit value at which concrete will not be damaged under the action of thermal fatigue is 0.2 to 0.4 times the ultimate tensile strain of the concrete material for C40 to C80 concrete.
[0071] Example 2
[0072] Based on the above embodiments, in a specific embodiment, a method for designing a temperature-adaptive elastic concrete composite structure includes the following steps:
[0073] S21: Clarify the meteorological data of the environment where the concrete structure is located and obtain the monthly average day and night temperature difference of the area;
[0074] S22: Determine the actual size of the concrete structure, conventional concrete pouring mix ratio and basic mechanical properties;
[0075] S23: Import the field parameters in S21 and S22 into the finite element analysis system, and use the independently developed temperature stress transfer model and temperature fatigue cumulative damage model to calculate the cracking location, maximum cracking depth and initial cracking time of the concrete structure;
[0076] S24: determining the mix ratio of the temperature-adaptive elastic concrete according to the relationship between the preset mix ratio of the temperature-adaptive concrete and the first crack time;
[0077] S25: Taking the maximum depth of damage to the concrete structure within the service life (i.e. the maximum value of the maximum cracking depth) as the dividing line, the barrier between the thermostatically adaptive elastic concrete and the conventional concrete is determined, and a "rigid inside and extended outside" thermostatically adaptive elastic concrete composite structure is designed, with the outer layer made of thermostatically adaptive elastic concrete and the inner layer made of conventional concrete.
[0078] Furthermore, the basic principle of the temperature stress transfer model is that in a large temperature difference environment, concrete generates a temperature gradient under the action of the ambient temperature difference and the local temperature difference of the concrete. During the temperature gradient change process, the contraction and expansion of the concrete structure are restricted, thereby generating self-constrained temperature stress and surface temperature stress, as shown below:
[0079]
[0080] Where a is the linear expansion coefficient of concrete (℃-1); ΔT 1 (t) is the temperature difference between the center and surface of concrete (℃); K(t,τ) is the stress relaxation coefficient of concrete; E(t) represents the elastic modulus of concrete; t is the stress generation time (s); τ is the stress retention time (s); ΔT 2 (t) is the reduction of comprehensive temperature difference of concrete; R(t) is the generalized constraint coefficient; C X is the external constraint horizontal deformation stiffness (N·m -3 ), H is the thickness of the concrete structure (m), and L is the length of the concrete structure (m).
[0081] Furthermore, the basic principle of the temperature fatigue cumulative damage model is that the temperature stress generated by the temperature gradient inside and outside the concrete structure under the action of the day and night temperature cycle increases and decreases periodically, and the temperature fatigue stress causes the internal damage of the concrete structure to gradually accumulate until it reaches a certain limit and causes the concrete structure to crack; the temperature fatigue cumulative damage model is expressed as the damage variable Dc:
[0082]
[0083] Where, dD c is the increment of fatigue damage; du m is the deformation increment; u m is the deformation; u ε is the cumulative deformation under temperature fatigue; T is the current stress increment; ft is the initial maximum normal stress; δ 0 is the deformation threshold; C f is the correction factor (0 <Cf<1)。
[0084] Furthermore, if cracking occurs in concrete structures under thermal fatigue stress, the following criteria should be met simultaneously:
[0085] Failure occurs only when the strain exceeds the ultimate tensile strain of concrete;
[0086] The degree of damage increase depends on the change of concrete strain. When the damage variable reaches a certain threshold, concrete will crack.
[0087] There is a certain limit value for the strain of concrete under temperature fatigue. Once the strain is lower than this limit value, the material will not suffer fatigue failure no matter how many times it cycles.
[0088] Furthermore, for C40-C80 concrete, the damage variable threshold for concrete cracking is that the concrete will only crack when the damage variable reaches 0.2-0.3.
[0089] Furthermore, the strain limit value at which concrete will not be damaged under the action of thermal fatigue is 0.2 to 0.4 times the ultimate tensile strain of the concrete material for C40 to C80 concrete.
[0090] Furthermore, the maximum depth boundary line of damage to the concrete structure within the service life is defined as a closed curve consisting of positions where the internal damage variable of the concrete structure within the design service life is 0.
[0091] Example 3
[0092] Based on the above embodiments, in a specific embodiment, a temperature-adaptive elastic concrete includes cement, machine-made sand, 5mm-10mm graded crushed stone, 10mm-20mm graded crushed stone, group A waterborne polyurethane, group B waterborne polyurethane, water-reducing and defoaming functional components and water.
[0093] Furthermore, the dosage of the raw material components of the temperature-adaptive elastic concrete is: cement 300kg / m 3 ~600kg / m 3 , Machine-made sand 400kg / m 3 ~800kg / m 3 , 5mm~10mm graded crushed stone 300kg / m 3 ~700kg / m 3 , 10mm~20mm graded crushed stone 400kg / m 3 ~800kg / m 3 、Group A waterborne polyurethane 10kg / m 3 ~50kg / m 3 、Group B waterborne polyurethane 5kg / m 3 ~25kg / m 3 , water-reducing and defoaming functional components 0kg / m 3 ~50kg / m 3 、Water 50kg / m 3~200kg / m 3 .
[0094] Furthermore, the adaptive group A water-based polyurethane is mainly prepared from the following raw materials in parts by weight: 30 to 80 parts of macromolecular diols, 30 to 60 parts of hydrophilic chain extenders, 1 to 10 parts of ethylene oxide, 1 to 5 parts of organic tin compounds, and 1 to 5 parts of antioxidants; the adaptive group B water-based polyurethane is mainly prepared from the following raw materials in parts by weight: 60 to 90 parts of diisocyanates, 10 to 20 parts of organic amine compounds and other raw materials.
[0095] Example 4
[0096] Based on the above embodiments, in a specific embodiment, a variable temperature self-adaptive elastic concrete composite structure includes an outer layer structure and an inner layer structure, wherein the outer layer structure is made of variable temperature self-adaptive elastic concrete.
[0097] Furthermore, the temperature-adaptive elastic concrete includes cement, machine-made sand, 5mm-10mm graded crushed stone, 10mm-20mm graded crushed stone, group A waterborne polyurethane, group B waterborne polyurethane, water-reducing and defoaming functional components and water.
[0098] Furthermore, the dosage of the raw material components of the temperature-adaptive elastic concrete is: cement 300kg / m 3 ~600kg / m 3 , Machine-made sand 400kg / m 3 ~800kg / m 3 , 5mm~10mm graded crushed stone 300kg / m 3 ~700kg / m 3 , 10mm~20mm graded crushed stone 400kg / m 3 ~800kg / m 3 、Group A waterborne polyurethane 10kg / m 3 ~50kg / m 3 、Group B waterborne polyurethane 5kg / m 3 ~25kg / m 3 , water-reducing and defoaming functional components 0kg / m 3 ~50kg / m 3 、Water 50kg / m 3 ~200kg / m 3 .
[0099] Furthermore, the adaptive group A water-based polyurethane is mainly prepared from the following raw materials in parts by weight: 30 to 80 parts of macromolecular diols, 30 to 60 parts of hydrophilic chain extenders, 1 to 10 parts of ethylene oxide, 1 to 5 parts of organic tin compounds, and 1 to 5 parts of antioxidants; the adaptive group B water-based polyurethane is mainly prepared from the following raw materials in parts by weight: 60 to 90 parts of diisocyanates, 10 to 20 parts of organic amine compounds and other raw materials.
[0100] Furthermore, the inner structure is made of conventional concrete.
[0101] Example 5
[0102] Based on the above embodiment, in a specific embodiment, the steps of designing the parameters of the temperature-adaptive elastic concrete composite structure are as follows:
[0103] S31: The environmental characteristics of area A obtained from the survey are as follows: annual average temperature -0.3℃; annual average daily temperature difference 25.8℃; solar radiation intensity 26136kJ / (m 2 d) Therefore, the highest and lowest temperatures of the daily temperature cycle are set in the finite element analysis software to be 15°C and -10°C respectively, and the temperature cycle adopts a constant amplitude sine wave with one cycle every 24 hours;
[0104] S32: It is clarified that the compressive and tensile strengths of conventional C40 railway bridge pier concrete are 61.53MPa and 10.78MPa respectively, and the elastic modulus is 44.92GPa, which are used as the material parameters of railway bridge pier concrete;
[0105] S33: Import the thermal fatigue cumulative damage model to perform finite element analysis on the concrete structure of the railway pier in area A;
[0106] S34: Analyze the simulation results, such as Figure 3 and Figure 4 As shown by Figure 3 It can be seen that the cracked part of the concrete structure of the railway pier in area A is located at the intersection of the arc and the plane at the bottom of the pier; Figure 4 It can be seen that the maximum damage depth (the depth corresponding to the damage variable Dc being 0) of the concrete structure of the railway pier with a design service life of 60 years is 17m, which is about 2 / 5 of the total radius;
[0107] S35: Based on the finite element analysis results, the design mix ratio of high crack-resistant elastic concrete is as follows: 1m 3 The raw materials contained are: 430kg cement; 604kg machine-made sand; 330kg 5mm-10mm gravel; 770kg 10mm-20mm gravel; 14.33kg group A water-based polyurethane; 7.17kg group B water-based polyurethane; 0.5kg water-reducing and defoaming functional component; 161kg water.
[0108] S36: Based on the analysis results, the dividing line is determined according to the maximum damage depth, the ratio of the outer layer to the inner layer is obtained, and it is determined that the high crack-resistant concrete composite structure of the railway bridge pier in area A should be designed with a ratio of external high crack-resistant elastic concrete to internal conventional concrete of 4:6.
[0109] Example 6
[0110] Based on the above embodiment, in a specific embodiment, the steps of designing the parameters of the temperature-adaptive elastic concrete composite structure are as follows:
[0111] S41: The environmental characteristics of area B obtained from the survey are as follows: annual average temperature 1.3℃; annual average daily temperature difference 15.8℃; solar radiation intensity 135629kJ / (m 2 d) Therefore, the highest and lowest temperatures of the daily temperature cycle are set to 15°C and 0°C respectively in the finite element analysis software. The temperature cycle adopts a constant amplitude sine wave with one cycle every 24 hours;
[0112] S42: It is clarified that the compressive and tensile strengths of conventional C40 railway bridge pier concrete are 55.83 MPa and 8.62 MPa respectively, and the elastic modulus is 41.32 GPa, which are used as the material parameters of railway bridge pier concrete;
[0113] S43: Import the thermal fatigue cumulative damage model to perform finite element analysis on the concrete structure of the railway pier in area B;
[0114] S44: Analyze the simulation results, such as Figure 5 and Figure 6 As shown by Figure 5 It can be seen that the cracked part of the concrete structure of the railway pier in area B is located at the intersection of the arc and the plane at the bottom of the pier; Figure 6 It can be seen that the maximum damage depth (corresponding to the depth when the damage variable Dc is 0) of the concrete structure of the railway pier with a design service life of 60 years is 9m, which is about 1 / 5 of the total radius;
[0115] S45: Based on the results of finite element analysis, the design mix ratio of raw materials for high crack-resistant elastic concrete is as follows: 430kg cement; 604kg machine-made sand; 330kg 5mm-10mm crushed stone; 770kg 10mm-20mm crushed stone; 28.67kg group A waterborne polyurethane; 14.33kg group B waterborne polyurethane; 0.3kg water-reducing and defoaming functional component; 151kg water.
[0116] S46: Based on the analysis results, it is determined that the high crack-resistant concrete composite structure of railway bridge piers in Nagqu area should be designed with a ratio of external high crack-resistant elastic concrete to internal conventional concrete of 2:8.
[0117] Example 7
[0118] Based on the above embodiment, in a specific embodiment, the steps of designing the parameters of the temperature-adaptive elastic concrete composite structure are as follows:
[0119] S51: The environmental characteristics of area C obtained from the survey are as follows: annual average temperature 0.6℃; annual average daily temperature difference 22.5℃; solar radiation intensity 20829kJ / (m 2 d) Therefore, the highest and lowest temperatures of the daily temperature cycle are set to 20°C and 0°C in the finite element analysis software. The temperature cycle is simplified by using a constant amplitude sine wave, with one cycle every 24 hours;
[0120] S52: It is clarified that the compressive and tensile strengths of conventional C40 railway bridge pier concrete are 56.32MPa and 9.41MPa respectively, and the elastic modulus is 42.38GPa, which are used as the material parameters of railway bridge pier concrete;
[0121] S53: Import the thermal fatigue cumulative damage model to perform finite element analysis on the concrete structure of the railway pier in area C;
[0122] S54: Analyze the simulation results, such as Figure 7 and Figure 8 As shown by Figure 7 It can be seen that the cracked part of the concrete structure of the railway pier in area C is located at the intersection of the arc and the plane at the bottom of the pier; Figure 8 It can be seen that the maximum damage depth (the depth corresponding to the damage variable Dc being 0) of the concrete structure of the railway pier with a design service life of 60 years is 13m, which is about 3 / 10 of the total radius;
[0123] S55: Based on the results of finite element analysis, the design mix ratio of raw materials for high crack-resistant elastic concrete is as follows: 430kg cement; 604kg machine-made sand; 330kg 5mm-10mm crushed stone; 330kg 10mm-20mm crushed stone; 43.00kg group A water-based polyurethane; 21.50kg group B water-based polyurethane; 0.2kg water-reducing and defoaming functional component; 140kg water.
[0124] S56: Based on the analysis results, it is determined that the high crack-resistant concrete composite structure of the railway bridge piers in area C should be designed with a ratio of external high crack-resistant elastic concrete to internal conventional concrete of 3:7.
[0125] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.
[0126] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for designing temperature-adaptive elastic concrete, characterized in that: The determination of the content of each component of the temperature-adaptive elastic concrete includes the following steps: Step 11: Collect ambient temperature difference data; Step 12: Obtain the actual size of the concrete structure, conventional concrete pouring mix ratio and basic mechanical performance indicators of the concrete structure; Step 13: According to the actual size of the concrete structure, the conventional concrete pouring mix ratio and the basic mechanical performance index of the concrete structure, a concrete structure model is constructed using a finite element analysis system, and a temperature deformation model is obtained by combining a temperature stress transfer model and a temperature fatigue cumulative damage model; the ambient temperature difference data is input into the temperature deformation model to obtain the first crack time of the concrete structure model; Step 14: Determine the mix ratio of the temperature-adaptive elastic concrete according to the mapping relationship between the mix ratio of the temperature-adaptive concrete and the first crack time.
2. A temperature-adaptive elastic concrete design method according to claim 1, characterized in that: The local temperature difference of concrete corresponding to the ambient temperature difference is obtained according to the ambient temperature difference data and the concrete structure model; the temperature stress transfer model represents the self-constrained temperature stress σ of the concrete structure model in the temperature gradient change process generated by the ambient temperature difference and the local temperature difference of concrete. Z (t) and surface temperature stress σ X (t), expressed as: Wherein, a is the linear expansion coefficient of the concrete structure; ΔT1(t) is the temperature difference between the center and the surface of the concrete structure obtained according to the ambient temperature difference data and the concrete structure model; K(t,τ) is the stress relaxation coefficient of the concrete structure; E(t) represents the elastic modulus of concrete; t is the stress generation time; τ is the stress retention time; ΔT2(t) is the comprehensive temperature difference reduction of the concrete structure obtained according to the ambient temperature difference data and the concrete structure model; R(t) is the generalized constraint coefficient; C X is the external constraint horizontal deformation stiffness; H is the thickness of the concrete structure; L is the length of the concrete structure.
3. A temperature-adaptive elastic concrete design method according to claim 1, characterized in that: The local temperature difference of concrete corresponding to the ambient temperature difference is obtained according to the ambient temperature difference data and the concrete structure model; the temperature fatigue cumulative damage model represents the damage variable Dc generated by the gradual accumulation of internal damage of the concrete structure by the temperature fatigue stress during the temperature gradient change process generated by the ambient temperature difference and the local temperature difference of concrete. The gradual accumulation of damage is represented by the fatigue damage increment, which is expressed as: Among them, dD c is the fatigue damage increment; du m is the deformation increment; u m is the deformation; u ε is the cumulative deformation under temperature fatigue; T is the current stress increment; ft is the initial maximum normal stress; δ0 is the deformation threshold; C f is the correction factor, 0 <C f <1.
4. A temperature-adaptive elastic concrete design method according to claim 3, characterized in that: In step 13, when the damage variable reaches the damage variable threshold and the strain value of the concrete structure reaches the ultimate tensile strain threshold, the concrete structure model cracks; the damage variable threshold is set to 0.2 to 0.3; the ultimate tensile strain threshold is set to 0.2 to 0.4 times.
5. A method for designing a temperature-adaptive elastic concrete composite structure, characterized in that: The following steps are involved: Step 21: Collecting ambient temperature difference data; Step 22: Obtain the actual size of the concrete composite structure, the conventional concrete pouring mix ratio and the basic mechanical performance indicators of the concrete structure; Step 23: According to the actual size of the concrete composite structure, the conventional concrete pouring mix ratio and the basic mechanical performance index of the concrete structure, a concrete structure model is constructed using a finite element analysis system, and a temperature deformation model is obtained by combining a temperature stress transfer model and a temperature fatigue cumulative damage model; the ambient temperature difference data is input into the temperature deformation model to obtain the maximum cracking depth and the initial cracking time of the concrete structure model; Step 24: determining the mix ratio of the temperature-adaptive elastic concrete according to the mapping relationship between the mix ratio of the temperature-adaptive concrete and the first crack time; Step 25: Select the maximum cracking depth within a preset period of time to determine a dividing line, determine the proportion of the variable temperature self-adaptive elastic concrete in the concrete composite structure according to the dividing line, and construct the variable temperature self-adaptive elastic concrete composite structure.
6. A temperature-adaptive elastic concrete, characterized in that: It includes cement, machine-made sand, 5mm-10mm graded crushed stone, 10mm-20mm graded crushed stone, group A water-based polyurethane, group B water-based polyurethane, water-reducing and defoaming functional components and water.
7. The temperature-adaptive elastic concrete according to claim 6, characterized in that: The content of each component is: cement 300kg / m 3 ~600kg / m3, machine-made sand 400kg / m 3 ~800kg / m 3 , 5mm~10mm graded crushed stone 300kg / m 3 ~700kg / m 3 , 10mm~20mm graded crushed stone 400kg / m 3 ~800kg / m3, Group A waterborne polyurethane 10kg / m 3 ~50kg / m 3 、Group B waterborne polyurethane 5kg / m 3 ~25kg / m 3 , water-reducing and defoaming functional components 0kg / m 3 ~50kg / m 3 、Water 50kg / m 3 ~200kg / m 3 .
8. A temperature-adaptive elastic concrete composite structure, characterized in that: A method for designing a temperature-adaptive elastic concrete composite structure as described in claim 5 is adopted, wherein the temperature-adaptive elastic concrete composite structure comprises an outer layer structure and an inner layer structure, and the outer layer structure adopts temperature-adaptive elastic concrete.
9. The temperature-adaptive elastic concrete composite structure according to claim 8, characterized in that: The variable temperature self-adaptive elastic concrete includes cement, machine-made sand, 5mm-10mm graded crushed stone, 10mm-20mm graded crushed stone, group A waterborne polyurethane, group B waterborne polyurethane, water-reducing and defoaming functional components and water.
10. The temperature-adaptive elastic concrete composite structure according to claim 8, characterized in that: Temperature adaptive elastic concrete including cement 300kg / m 3 ~600kg / m3, machine-made sand 400kg / m 3 ~800kg / m 3 , 5mm~10mm graded crushed stone 300kg / m 3 ~700kg / m 3 , 10mm~20mm graded crushed stone 400kg / m 3 ~800kg / m3, Group A waterborne polyurethane 10kg / m 3 ~50kg / m 3 、Group B waterborne polyurethane 5kg / m 3 ~25kg / m 3 , water-reducing and defoaming functional components 0kg / m 3 ~50kg / m 3 、Water 50kg / m 3 ~200kg / m 3 .
Citation Information
Patent Citations
Heat-sensitive material modified concrete, prefabricated part of modified concrete and preparation method for cast-in-place of modified concrete
CN103936367A
Mass concrete temperature control optimization method
CN110728093A
Ballastless track self-compacting concrete fatigue damage calculation method
CN114547734A
Ballastless track roadbed slab concrete anti-cracking control method
CN116674052A
Curing method for cement concrete
JP2016094743A
Cited By
A multi-component synergistic fatigue-resistant concrete for high-altitude environments and its preparation method
CN123106121A