Glass fiber needle felt and preparation method thereof
Through the method of acid leaching and sintering, the problem of cumbersome preparation and uneven silicon oxide content in the preparation of glass fiber needle felt was solved, and efficient and low-damage glass fiber needle felt preparation was achieved, which improved the strength and finished product rate. .
Patent Information
- Application Number
- CN202211351743.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-10-31
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2042-10-31
AI Technical Summary
The existing glass fiber needle felt preparation process has problems such as cumbersome preparation, uneven silicon oxide content, large fiber damage, low strength and low yield.
After acid leaching and washing, the glass fibers are cut into chopped fibers, and the moisture content is controlled to be 1 to 6 wt%, loosen, comb into a net, needle puncture, and sintering on the bottom material to reduce thermal sintering shrinkage Tension, achieve efficient preparation of glass fiber needle felt.
The production efficiency of glass fiber needle felt is improved, the fiber damage is small, the strength is high, and the yield is high, and the fluctuations in the silicon oxide content and mechanical damage during thermal sintering are avoided, and the apparent quality is good.
Smart Images

Figure CN116065300B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of glass fibers, and in particular to a glass fiber needle felt and a preparation method thereof. Background Art
[0002] Glass fiber needle felt is a felt-like non-woven filter material made of glass fiber as raw material. The fiber fibers between the felt layer and between the felt layer and the reinforced glass fiber base cloth are entangled mechanically to reinforce the fiber mesh. Common glass fiber needle felts include medium silica glass fiber needle felt and high silica glass fiber needle felt. Among them, high silica glass fiber is a high-temperature resistant inorganic fiber material with excellent properties such as high temperature resistance, wave transmission, and light weight. It has been widely used in high-temperature thermal insulation protection and wave transmission, thermal insulation protection materials and other fields of aerospace vehicles. Glass fiber needle felt is made of high silica glass fiber chopped yarn through a special process. It is widely used in chemical pipeline insulation, energy saving and carbon reduction, thermal insulation, sound absorption, flame retardancy, flue gas filtration in the automotive industry, high-temperature filtration of metallurgical building materials and other fields. Energy conservation and carbon reduction are becoming increasingly stringent. As an environmentally friendly and energy-saving thermal insulation multifunctional material, glass fiber needle felt does not contain organic matter, does not burn or smoke in high-temperature environments, is pollution-free, and has a low thermal conductivity, playing an important role in the field of energy conservation and carbon reduction.
[0003] Chinese patent CN03222687.X discloses using special equipment to comb, lay nets, and then needle punch to obtain needle felt, and then acid leaching to obtain glass fiber needle felt. However, the glass fiber needle felt prepared by this method will become loose during the acid washing process, and the silicon oxide content is uneven, which seriously affects its quality.
[0004] Chinese patent CN201610280109.4 discloses a method for preparing a high temperature resistant filter felt, which first prepares a high-silica fiber by subjecting the glass fiber to an acid treatment and a heat sintering process, and then prepares a glass fiber needle felt by combing, web forming and needle punching the short glass fiber bundles, and then forms a high temperature resistant filter felt after impregnation treatment and curing and shaping. However, the preparation process is cumbersome, inefficient and costly. Summary of the invention
[0005] The embodiment of the present invention provides a glass fiber needle felt and a preparation method thereof. The preparation method has high production efficiency and the prepared glass fiber needle felt has small fiber damage, high strength and high yield.
[0006] In a first aspect, the present invention provides a method for preparing a glass fiber needle felt, the preparation method comprising the following steps:
[0007] The glass fiber is acid-leached and water-washed to obtain a wet-state base fiber;
[0008] Cutting the wet base fiber into short-cut fibers, and drying the short-cut fibers to obtain short-cut fibers with a moisture content of 1 to 6 wt %;
[0009] The short-cut fibers with a moisture content of 1 to 6 wt % are sequentially opened, carded into a web, and needled to obtain a needle-punched felt;
[0010] The needle-punched felt is placed on a base material, and the needle-punched felt and the base material are sintered to obtain the glass fiber needle-punched felt.
[0011] Preferably, the glass fiber includes at least one of alkali-free glass fiber, binary glass fiber, and ternary glass fiber.
[0012] Preferably, the diameter of the glass fiber is 4-11 μm.
[0013] More preferably, the length of the glass fiber does not exceed 11 cm.
[0014] Preferably, the glass fiber is a loose raw fiber bundle obtained by cutting and loosening a raw fiber cake; preferably, the width of the loose raw fiber bundle is 2 to 3 times the width of the raw fiber cake.
[0015] Preferably, the silicon oxide content of the wet-state base fiber is not less than 85 wt %.
[0016] Preferably, the silicon oxide content of the wet-state base fiber is not less than 92 wt%.
[0017] Preferably, the silicon oxide content of the wet-state base fiber is not less than 96 wt %.
[0018] Preferably, the moisture content of the wet-state base fiber is 10-15wt%.
[0019] Preferably, the length of the chopped fibers is 50 to 130 mm.
[0020] More preferably, the length of the chopped fibers is 80 to 110 mm.
[0021] Preferably, the drying is carried out by microwave drying and hot air circulation drying;
[0022] The drying temperature is 110-130°C.
[0023] More preferably, after the drying, the chopped fibers have a moisture content of 2 to 4 wt %.
[0024] Preferably, the carded web is laid using a double-layer web.
[0025] Preferably, the acupuncture includes pre-puncture and main puncture.
[0026] Preferably, the sintering process adopts horizontal sintering;
[0027] The bottom supporting material comprises a sheet material with a temperature resistance of 700 to 1000°C.
[0028] More preferably, the sheet material is high-silica glass fiber cloth or high-silica glass fiber mesh cloth.
[0029] Preferably, the length ratio of the needle felt to the base material is (1-1.2):1.
[0030] In a second aspect, the present invention further provides a glass fiber needle-punched felt prepared by any of the preparation methods provided in the first aspect.
[0031] Compared with the prior art, the present invention has at least the following beneficial effects:
[0032] The present invention prepares wet-state base fibers by acid leaching glass fibers, controls the moisture content of the fibers to be 1-6 wt% after short cutting and drying, and then loosens, combs into a web, and needles the fibers to obtain a needled felt, and then sintering the needled felt to prepare a glass fiber needled felt. The preparation method not only has high combing efficiency, small fiber damage, high needled felt strength, and high yield, but also avoids the disadvantages of the prior art such as complicated preparation, large fluctuation of silicon oxide content, large fiber damage caused by combing, low needled felt strength, and low yield.
[0033] In the present invention, during the sintering process, the needle felt is placed on a base material and sintered together with the base material. The base material allows the needle felt to be sintered at high temperature without being stressed, thereby achieving "static" sintering and reducing the mechanical damage caused by the dual effects of fiber shrinkage tension during thermal sintering and cloth roll tension. This reduces the strength loss of the needle felt during the thermal sintering process and retains the mechanical properties of the needle felt.
[0034] The present invention can be designed to prepare medium-silica glass fiber needle felt (silicon oxide content is 85-92wt%) and high-silica glass fiber needle felt (silicon oxide content is not less than 96wt%) as required, and its surface quality is good without surface cracks and depressions. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Figure 1 This is a flow chart of a method for preparing a glass fiber needle felt provided by an embodiment of the present invention;
[0036] Figure 2 This is a physical picture of the high-silica glass fiber needle-punched felt product provided in Example 1 of the present invention;
[0037] Figure 3 This is a physical picture of a high-silica glass fiber needle-punched felt product provided in Example 1 of the present invention. DETAILED DESCRIPTION
[0038] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention and the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0039] The present invention provides a method for preparing a glass fiber needle felt. Figure 1 As shown, the preparation method comprises the following steps:
[0040] Step (1): acid leaching and water washing the glass fiber to obtain wet base fiber;
[0041] Step (2): cutting the wet base fiber into short-cut fibers, and drying the short-cut fibers to obtain short-cut fibers having a moisture content of 1 to 6 wt %;
[0042] Step (3): opening, combing and needle-punching the chopped fibers with a moisture content of 1 to 6 wt % in sequence to obtain a needle-punched felt;
[0043] Step (4): placing the needle-punched felt on a base material, and sintering the needle-punched felt together with the base material to obtain a glass fiber needle-punched felt.
[0044] According to some preferred embodiments, the glass fiber includes at least one of alkali-free glass fiber, binary glass fiber, and ternary glass fiber.
[0045] It should be noted that at least one is any one or a mixture of any several in any proportion.
[0046] According to some preferred embodiments, the diameter of the glass fiber is 4 to 11 μm (for example, 4 μm, 4.5 μm, 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, 8.5 μm, 9 μm, 9.5 μm, 10 μm, 10.5 μm or 11 μm).
[0047] In the present invention, it has been experimentally confirmed that if the diameter of the glass fiber is too small or too large, it is not conducive to the acid leaching process. Therefore, the diameter of the glass fiber selected in the present invention is 4 to 11 μm.
[0048] According to some more preferred embodiments, the length of the glass fiber does not exceed 11 cm (for example, it may be 11 cm, 10 cm, 8 cm, 7 cm, 6 cm or 5 cm, etc.).
[0049] According to some preferred embodiments, the glass fiber is a loose raw fiber bundle obtained by cutting and opening raw fiber cakes.
[0050] It should be noted that the glass fibers are all raw fibers, that is, the raw fibers are bundled into fibers by a bundler after drawing and forming, and have not been processed by processes such as annealing.
[0051] According to some more preferred embodiments, the width of the loose raw silk bundle is 2 to 3 times (for example, it can be 2 times, 2.5 times or 3 times) the width of the raw silk cake.
[0052] Specifically, the present invention uses a raw silk cake drawn into a fiber diameter of 4 to 11 μm, and then cuts to obtain a long glass fiber bundle with a length not exceeding 11 cm, and then opens and draws the long glass fiber bundle into a loose raw silk bundle according to 2 to 3 times the width of the raw silk cake, so that the single-filament bundle is evenly dispersed and thus facilitates a fully and evenly acid leaching treatment. It should be noted that when the glass fiber is composed of alkali-free glass fiber, binary glass fiber and ternary glass fiber, the above three raw silk cakes can be opened into loose raw silk bundles and mixed, and then acid leached and washed together.
[0053] The present invention directly adopts raw silk cakes, cuts and loosens the raw silk cakes to obtain mesh raw silk for acid leaching without debonding, directly omitting these two process steps, shortening the preparation cycle and improving production efficiency.
[0054] According to some preferred embodiments, the silicon oxide content of the wet-based fiber is not less than 85 wt % (for example, it may be 85 wt %, 88 wt %, 90 wt %, 92 wt %, 95 wt %, 96 wt %, 97 wt %, etc.).
[0055] According to some preferred embodiments, the silicon oxide content of the wet-based fiber is not less than 92 wt % (for example, it may be 92 wt %, 93 wt %, 95 wt %, 96 wt %, 97 wt %, etc.).
[0056] According to some more preferred embodiments, the silicon oxide content of the wet-based fiber is not less than 96 wt % (for example, it may be 96 wt %, 96.5 wt %, 97 wt %, 97.5 wt %, 98 wt %, etc.).
[0057] The present invention can be designed and prepared according to demand to prepare medium-silica glass fiber needle felt (silicon oxide content is 85-92wt%), high-silica glass fiber needle felt (silicon oxide content is not less than 96wt%)
[0058] According to some preferred embodiments, the moisture content of the wet-based fiber is 10-15 wt% (for example, 10 wt%, 11 wt%, 12 wt%, 13 wt%, 14 wt% or 15 wt%).
[0059] It should be noted that the moisture content of the wet-based fiber obtained after acid leaching and water washing is 10-15wt%. However, if the glass fiber with this moisture content is combed into a web, it will seriously affect the combing efficiency and even the quality of the web. Therefore, it is necessary to further control its moisture content by drying.
[0060] According to some preferred embodiments, the length of the chopped fibers is 50 to 130 mm (for example, 50 mm, 55 mm, 60 mm, 65 mm, 70 mm, 75 mm, 80 mm, 90 mm, 100 mm, 110 mm, 115 mm, 120 mm, 125 mm or 130 mm).
[0061] According to some more preferred embodiments, the length of the chopped fibers is 80 to 110 mm (e.g., 80 mm, 85 mm, 90 mm, 95 mm, 100 mm, 105 mm, or 110 mm).
[0062] In step (2) of the present invention, it has been experimentally confirmed that if the length of the short-cut fibers is too short or too long, it is not conducive to carding into a web and will affect the carding efficiency. Secondly, if the length of the short-cut fibers is too short, it will also affect the strength of the prepared glass fiber needle felt; if the length of the short-cut fibers is too long, it will also damage the appearance and uniformity of the glass fiber needle felt and even affect its filtering performance.
[0063] According to some preferred embodiments, the drying is carried out by microwave drying and hot air circulation drying;
[0064] The drying temperature is 110-130° C. (for example, 110° C., 115° C., 120° C., 125° C., or 130° C.).
[0065] The present invention adopts microwave drying and hot air circulation drying for drying in step (2), which can further shorten the drying time, realize rapid drying of the chopped fibers, and control the moisture content of the chopped fibers after drying to 1 to 6wt% (for example, it can be 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt%, 5wt%, 5.5wt% or 6wt%).
[0066] According to some more preferred embodiments, after drying, chopped fibers having a moisture content of 2 to 4 wt% (for example, 2 wt%, 2.2 wt%, 2.5 wt%, 2.8 wt%, 3 wt%, 3.2 wt%, 3.5 wt%, 3.8 wt% or 4 wt%) are obtained.
[0067] It should be noted that the carding machine is mainly composed of a pricking stick, a cylinder, a working roller and a doffer, which can finely comb, peel and web the chopped fibers, and then transmit the fiber web to the next process through the doffer and rollers. In the present invention, it has been experimentally confirmed that the control of moisture content is the key to carding and web formation. When the moisture content of the chopped fibers is greater than 6wt%, the chopped fibers form hair balls at the pricking stick and adhere to the pricking stick, and the fibers cannot be further loosened. The cylinder will also adhere to a large amount of cotton fibers, and the web cannot be formed; and when the moisture content of the chopped fibers is lower than 1wt%, the chopped fibers show a brittle fracture phenomenon and generate static electricity, causing the fibers to be entangled on the rollers, and the fibers cannot be further loosened, resulting in the inability to form a web. More importantly, the inventors found that when the moisture content of the chopped fibers is controlled at 2-4wt%, the rotation speed of the cylinder can be increased to 700-1000rpm, while the rotation speed of the cylinder in the existing preparation process is 500-600rpm. This not only significantly improves the carding efficiency, but also improves the uniformity of the carded web.
[0068] According to some preferred embodiments, the carded web is laid using a double layer.
[0069] It should be noted that the present invention can use a single-combing machine to form the web, but in order to obtain a more uniform web quality, it is preferably used with a double-combing machine to comb the cotton into the web, and then double-layer web laying to further improve the quality uniformity and controllability of the web laying.
[0070] According to some preferred embodiments, acupuncture includes pre-puncture and main puncture.
[0071] In the present invention, the density and depth of the needles can be designed according to the thickness of the needle felt, and the needle felt having both certain strength and firmness can be manufactured through the two processes of pre-puncturing and main puncturing.
[0072] According to some preferred embodiments, the sintering process adopts horizontal sintering;
[0073] The base material includes a sheet having a temperature resistance of 700 to 1000° C. (for example, 700° C., 750° C., 800° C., 850° C., 900° C., 950° C., or 1000° C.).
[0074] According to some more preferred embodiments, the sheet material is high-silica glass fiber cloth, high-silica glass fiber mesh cloth or high-temperature resistant ceramic fiber cloth, etc.
[0075] According to some preferred embodiments, the length ratio of the needle felt to the backing material is (1-1.2):1 (for example, it may be 1:1, 1.05:1, 1.1:1, 1.15:1 or 1.2:1).
[0076] According to some more preferred embodiments, the thickness of the base material may be 0.1 mm, 0.15 mm, 0.2 mm, 0.25 mm, 0.3 mm, 0.4 mm, 0.5 mm, 0.7 mm, 1 mm or even thicker.
[0077] In the present invention, in order to reduce the strength loss of the needle felt during the sintering process, a horizontal sintering furnace is used, and during the sintering process, the needle felt is placed on a base material and sintered together with the base material. The base material is used to make the needle felt sintered at high temperature without stress, thereby achieving "static" sintering (equivalent to the needle felt and the base material remaining relatively still), reducing the mechanical damage caused by the dual effects of the fiber thermal sintering shrinkage tension and the cloth roll tension, and retaining the mechanical properties of the needle felt.
[0078] It should be noted that since the base material will be stretched by traction, experiments have confirmed that the length ratio of the needle felt and the base material is (1-1.2):1, so as to ensure that during the continuous sintering process, the needle felt is not subject to traction tension during the forward process and can still be located on the base material, maintaining "static" sintering, avoiding the thermal shrinkage of the high silica felt and the pulling tension on the needle felt.
[0079] The present invention also provides a glass fiber needle-punched felt, which is prepared by any of the above-mentioned preparation methods.
[0080] The glass fiber needle-punched felt prepared by the present invention has good apparent quality, without surface cracks or dents, and the preparation process has high production efficiency throughout the entire process, little fiber damage, high needle-punched felt strength, and high yield, thereby avoiding the shortcomings of the prior art, such as complicated preparation, large fluctuations in silicon oxide content, large combed fiber damage, low needle-punched felt strength, and low yield.
[0081] In order to more clearly illustrate the technical solution and advantages of the present invention, a glass fiber needle felt and a preparation method thereof are described in detail below through several embodiments.
[0082] Example 1
[0083] (1) preparing a raw silk cake of alkali-free glass fiber with a fiber diameter of 4 to 11 μm, then cutting the raw silk cake to obtain a long glass fiber bundle with a length of 8 cm, and then opening and pulling the long glass fiber bundle into a loose raw silk bundle at a length of 2 to 3 times the width of the raw silk cake; using the loose raw silk bundle as glass fiber; acid leaching and water washing the glass fiber to obtain a wet-based fiber with a moisture content of 10 to 15 wt% and a silicon oxide content of 98 wt%;
[0084] (2) cutting the wet base fiber in step (1) into short fibers with a length of 50 to 130 mm, and drying them at 110° C. by microwave drying and hot air circulation drying to obtain short fibers with a moisture content of 2 wt %;
[0085] (3) the chopped fibers with a moisture content of 2 wt % in step (2) are opened in sequence, and are carded into a web using a double-layer web laying process, and are needled in two steps of pre-needling and main needling to obtain a needle-punched felt; wherein the rotation speed of the cylinder is 1000 rpm;
[0086] (4) using a horizontal sintering furnace, placing the needle-punched felt in step (3) on a base material (high-silica glass fiber cloth), and unwinding the needle-punched felt to base material at a length ratio of 1.1:1, so that the needle-punched felt and the base material are sintered together at 700° C. to obtain a high-silica glass fiber needle-punched felt.
[0087] Example 2
[0088] (1) preparing a raw silk cake of magnesium-aluminum-silicon high-strength and high-elastic glass fiber and a raw silk cake of alkali-free glass fiber with a fiber diameter of 4 to 11 μm, and then cutting each raw silk cake to obtain a long glass fiber bundle with a length of 8 cm, and then opening and pulling the long glass fiber bundle into a loose raw silk bundle at a width of 2 to 3 times of the raw silk cake; the loose raw silk bundle of magnesium-aluminum-silicon high-strength and high-elastic glass fiber and the loose raw silk bundle of alkali-free glass fiber are used as glass fibers in a mass ratio of 1:1; acid leaching and water washing the glass fibers to obtain wet-based fibers with a moisture content of 10 to 15 wt% and a silicon oxide content of 98 wt%;
[0089] (2) cutting the wet base fiber in step (1) into short fibers with a length of 50 to 130 mm, and drying them at 110° C. by microwave drying and hot air circulation drying to obtain short fibers with a moisture content of 2 wt %;
[0090] (3) the chopped fibers with a moisture content of 2 wt % in step (2) are opened in sequence, and combed into a web using a double-layer web laying process, and then needled in two steps of pre-needling and main needling to obtain a needle-punched felt;
[0091] (4) using a horizontal sintering furnace, placing the needle-punched felt in step (3) on a base material (high-silica glass fiber cloth), and unwinding the needle-punched felt to base material at a length ratio of 1.1:1, so that the needle-punched felt and the base material are sintered together at 700° C. to obtain a high-silica glass fiber needle-punched felt.
[0092] Example 3
[0093] Embodiment 3 is substantially the same as Embodiment 1, except that:
[0094] In step (2), the wet-based fibers in step (1) are cut into short-fiber glass fiber needle-punched mats having a length of 80 to 110 mm.
[0095] Example 4
[0096] Embodiment 4 is substantially the same as Embodiment 1, except that:
[0097] In step (2), microwave drying and hot air circulation drying are used at 130° C. to obtain short-cut fibers with a moisture content of 4 wt %.
[0098] Example 5
[0099] Embodiment 5 is substantially the same as Embodiment 1, except that:
[0100] In step (2), microwave drying and hot air circulation drying are used at 110° C. to obtain short-cut fibers with a moisture content of 1 wt %.
[0101] Example 6
[0102] Embodiment 6 is substantially the same as Embodiment 1, except that:
[0103] In step (2), microwave drying and hot air circulation drying are used at 110° C. to obtain short-cut fibers with a moisture content of 6 wt %.
[0104] Example 7
[0105] Embodiment 7 is substantially the same as Embodiment 1, except that:
[0106] In step (1), after acid leaching and water washing, wet base fibers with a moisture content of 10-15 wt% and a silicon oxide content of 88 wt% are obtained, and finally medium-silica glass fiber needle-punched felt is prepared.
[0107] Example 8
[0108] Embodiment 8 is substantially the same as Embodiment 1, except that:
[0109] In step (3), a single-layer web is used for carding.
[0110] Comparative Example 1
[0111] Comparative Example 1 is substantially the same as Example 1, except that:
[0112] The needle-punched felt in step (3) is directly sintered at 700° C. in a horizontal sintering furnace to obtain a high-silica glass fiber needle-punched felt.
[0113] Comparative Example 2
[0114] Comparative Example 2 is substantially the same as Example 1, except that:
[0115] In step (2), microwave drying and hot air circulation drying are used at 110° C. to obtain short-cut fibers with a moisture content of 10 wt %.
[0116] Comparative Example 3
[0117] Comparative Example 3 is substantially the same as Example 1, except that: the preparation process is different;
[0118] Specifically, a raw silk cake of alkali-free glass fiber with a fiber diameter of 4 to 11 μm is prepared, and then the raw silk cake is debonded, acid-leached, washed, sintered, chopped, combed into a web, and needle-punched to obtain a high-silica glass fiber needle-punched felt with a silicon oxide content of 98 wt%; wherein the rotation speed of the cylinder during the combing process is 500 rpm.
[0119] Comparative Example 4
[0120] Comparative Example 4 is substantially the same as Comparative Example 3, except that the rotation speed of the cylinder during the carding process is 1000 rpm.
[0121] The glass fiber needle punched felts prepared in Examples 1 to 8 and Comparative Examples 1 to 4 were used as samples for mechanical property tests, and the yield of the glass fiber needle punched felts prepared by the methods of the above Examples and Comparative Examples was tested, wherein the tensile strength, i.e., the yield, is shown in Table 1. Specifically, the tensile strength test method: the tensile breaking strength test was performed on the type II sample determined by the national standard GB / T 7689.5.
[0122] Table 1
[0123] Example Tensile strength(N) Yield rate (%) 1 105 90.0 2 110 89.1 3 106 89.5 4 105.5 90.2 5 104 89.6 6 105 90.0 7 103.5 89.8 8 99 89.3 Comparative Example 1 35 55.1 Comparative Example 2 31 35.0 Comparative Example 3 75 85.2 Comparative Example 4 63 80.6
[0124] It should be noted that since the moisture content of the chopped fibers in Comparative Example 2 is higher than 6wt%, when the chopped fibers form pills at the thorn and adhere to the thorn, the fibers cannot be further loosened, and a large amount of cotton fibers will also adhere to the cylinder, making it impossible to form a web; and in Comparative Example 4, due to the excessive rotation speed of the cylinder, a large amount of cotton fibers will adhere to the cylinder, making it difficult to form a web, and the yield is low.
[0125] Depend on Figure 2 and Figure 3 It can be seen that the glass fiber needle felt prepared by the present invention has good surface quality and no surface cracks or depressions. As shown in Table 1, the glass fiber needle felt prepared by the preparation method of the present invention significantly improves the yield of the glass fiber needle felt, and the preparation process is simple and suitable for large-scale batch production. At the same time, compared with the existing preparation process, the prepared glass fiber needle felt has less fiber damage and higher strength.
[0126] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit them; although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the above embodiments, or replace some of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present invention. The parts not described in detail in the present invention are well-known technologies of those skilled in the art.
Claims
1. A method for preparing a glass fiber needle felt, characterized in that: The preparation method comprises the following steps: The glass fibers are acid-leached and water-washed to obtain wet-state base fibers; the glass fibers are loose raw fiber bundles obtained by cutting and opening raw fiber cakes, and are not subjected to a debonding process; Cutting the wet base fiber into short-cut fibers, and drying the short-cut fibers to obtain short-cut fibers with a moisture content of 2-4 wt %; The short-cut fibers with a moisture content of 2-4 wt % are sequentially opened, carded into a web, and needled to obtain a needle-punched felt; The needle-punched felt is placed on a base material, and the needle-punched felt and the base material are sintered to obtain the glass fiber needle-punched felt; the length ratio of the needle-punched felt to the base material is (1-1.2):
1.
2. The preparation method according to claim 1, characterized in that: The glass fiber includes at least one of alkali-free glass fiber, binary glass fiber, and ternary glass fiber; and / or The diameter of the glass fiber is 4-11 μm, and the length of the glass fiber does not exceed 11 cm.
3. The preparation method according to claim 1, characterized in that: The width of the loose raw silk bundle is 2 to 3 times the width of the raw silk cake.
4. The preparation method according to claim 1, characterized in that: The silicon oxide content of the wet base fiber is not less than 85wt%; and / or The moisture content of the wet-based fiber is 10-15wt%.
5. The preparation method according to claim 1, characterized in that: The silicon oxide content of the wet-based fiber is not less than 92 wt %.
6. The preparation method according to claim 1, characterized in that: The silicon oxide content of the wet-based fiber is not less than 96 wt %.
7. The preparation method according to claim 1, characterized in that: The length of the chopped fibers is 50 to 130 mm; The drying temperature is 110-130°C.
8. The preparation method according to claim 1, characterized in that: The length of the chopped fibers is 80-110 mm.
9. The preparation method according to claim 1, characterized in that: The carding web is formed by double-layer web laying; and / or The acupuncture includes pre-puncture and main puncture.
10. The preparation method according to claim 1, characterized in that: The sintering process adopts horizontal sintering; The bottom supporting material comprises a sheet material with a temperature resistance of 700-1000° C.; the sheet material is a high-silica glass fiber cloth.
11. A glass fiber needle felt, characterized in that: The method is prepared by any one of claims 1 to 10.
Citation Information
Patent Citations
Preparation method of high-temperature-resistant filter felt
CN105879494A
High silica glass fiber punched felt
CN2633912Y
Basalt fiber high temperature compositing filter material
CN101053718A
Process for manufacturing multielement composition high silica glass fibre fixed-length yarn
CN102864542A