Process method for thinning back surface of wafer
By forming an annular invisible isolation belt on the back of the wafer to block stress transmission, the problem of intensified wafer edge damage is solved, and the reliability and yield of the product are improved.
Patent Information
- Application Number
- CN202411061165.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-19
AI Technical Summary
During the thinning process of wafer back, the damage to the edge of the wafer intensifies, affecting product reliability and yield.
After the film is applied on the front of the wafer, an annular invisible isolation belt is formed on the back of the wafer by invisible cutting through an annular laser to prevent the transmission of stress and prevent further expansion of damage.
Effectively reduce or avoid wafer edge damage and extend to effective products, improving product reliability and yield.
Smart Images

Figure CN118983214A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of integrated circuit manufacturing technology, and in particular to a process method for thinning the back side of a wafer. Background Art
[0002] The progress of integrated circuit manufacturing technology comes from the requirements of the market and competition. In the manufacturing and processing of wafers, a series of complex processes such as grinding, etching, cleaning, and polishing are often involved, so that the surface of the wafer can be processed into a specific integrated circuit structure. From the perspective of the cross-sectional structure of the integrated circuit, most integrated circuits are manufactured on the shallow surface layer of the wafer material. Due to the requirements of the manufacturing process, high requirements are placed on the dimensional accuracy, geometric accuracy, surface cleanliness, and surface microlattice structure of the wafer. Therefore, in hundreds of process flows, thinner wafers cannot be used, and only wafers of a certain thickness can be used for transfer and tape-out during the process. Usually, before the integrated circuit is packaged, a certain thickness of excess substrate material on the back of the wafer needs to be removed. This process is called the wafer back thinning process. Thinning the wafer by thinning not only improves the heat dissipation effect of the chip, but also thinning it to a certain thickness is beneficial to the later packaging process.
[0003] During the execution of various processes, including the process of wafer cutting from ingots, wafer handling and storage, wafer deposition or etching steps, wafer grinding or polishing, and thermal stress generated during wafer heating, it is possible to cause damage to the wafer edge, such as chipping, cracks, etc. On this basis, the process of thinning the back of the wafer will aggravate the damage to the wafer edge and deteriorate toward the inside of the wafer, affecting product reliability and reducing product yield. Summary of the invention
[0004] In view of the shortcomings of the prior art described above, the object of the present invention is to provide a process method for thinning the back side of a wafer, which is used to solve the problem in the prior art that the damage to the edge of the wafer will be aggravated during the thinning process of the back side of the wafer and deteriorate toward the inside of the wafer, affecting product reliability and reducing product yield.
[0005] To achieve the above-mentioned object and other related objects, the present invention provides a process for thinning the back side of a wafer, the process comprising:
[0006] Providing wafers with completed product front-side processes and attaching a film to the front side of the wafers;
[0007] Performing annular laser invisible cutting on the edge of the wafer from the back side of the wafer to form an annular invisible isolation zone at a preset depth inside the front edge of the wafer, and the invisible isolation zone at least partially extends in the thickness direction of the wafer to the area corresponding to the front process area of the product in the thickness direction of the wafer;
[0008] Performing backside thinning on the wafer to make the wafer reach a desired thickness;
[0009] The front side film of the wafer is removed.
[0010] Optionally, short pulse laser is used to perform ring-shaped laser invisible cutting on the edge of the wafer.
[0011] Optionally, the invisible isolation zone is an annular continuous invisible isolation zone.
[0012] Optionally, the shape of the invisible isolation zone is the same as that of the wafer, both of which are circular.
[0013] Furthermore, in the radial direction of the wafer, the distance between the invisible isolation zone and the outer peripheral edge of the wafer is 2.2 mm to 2.8 mm.
[0014] Optionally, a dual-axis process is used to thin the back side of the wafer.
[0015] Optionally, after removing the film on the front side of the wafer, the method further includes the steps of wet grinding the back side of the wafer and forming a metal electrode coating on the back side of the wafer.
[0016] Optionally, the thickness of the wafer is 700 μm to 750 μm, and the preset depth of the invisible isolation zone inside the front edge of the wafer is 10 μm to 300 μm.
[0017] Optionally, the width of the invisible isolation zone is 3 μm to 4 μm.
[0018] Optionally, part of the thickness of the invisible isolation zone extends into a region corresponding to the product front process area in the wafer thickness direction, and another part of the thickness extends into a region corresponding to the product front process area in the wafer thickness direction.
[0019] As described above, the process method for thinning the back side of the wafer of the present invention performs annular laser invisible cutting on the edge of the wafer from the back side of the wafer after the film is attached to the front side of the wafer and before the back side of the wafer is thinned, so as to form an annular invisible isolation belt at a preset depth inside the front edge of the wafer, and the invisible isolation belt at least partially extends into the area corresponding to the product front process in the wafer thickness direction in the wafer thickness direction. The invisible isolation belt can block the transmission of stress during the thinning process of the back side of the wafer, so that when the edge of the wafer is damaged during the process of the front side of the product, the further expansion of the damage can be blocked, that is, the damage of the edge of the wafer is blocked from further extending into the inside of the wafer, effectively reducing or even avoiding the extension of the damage of the edge of the wafer to the effective product, thereby improving product reliability and product yield. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 Shown is a schematic diagram of the top view of the structure of forming a ring-shaped invisible isolation zone by performing annular laser invisible cutting on the edge of the back side of the wafer in the process method for thinning the back side of the wafer of the present invention, wherein the invisible isolation zone is represented by a dotted line to indicate its position setting in the wafer.
[0021] Figure 2 Display as Figure 1 Schematic diagram of the cross-sectional structure along the AA direction.
[0022] Figure 3 The diagram shows an example of a top-down structure of a wafer after the back side of the wafer is thinned, wherein the damage on the edge of the wafer deteriorates toward the inside of the wafer after the back side of the wafer is thinned.
[0023] Component number description
[0024] 10 Wafer
[0025] 11 Invisible isolation belt
[0026] 12 Hidden Crack
[0027] 13 Product front process area DETAILED DESCRIPTION
[0028] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0029] See also Figures 1 to 3 It should be noted that the illustrations provided in this embodiment are only used to illustrate the basic concept of the present invention in a schematic manner, and the illustrations only show components related to the present invention rather than being drawn according to the number, shape and size of components in actual implementation. In actual implementation, the type, quantity and proportion of each component may be changed arbitrarily, and the component layout may also be more complicated.
[0030] As described in the background technology, during the execution of various processes on the front side of the wafer product, including the process of cutting the wafer from the ingot, the process of transporting and storing the wafer, the deposition or etching step of the wafer, the grinding or polishing process of the wafer, the thermal stress generated during the heating process of the wafer, etc., it is possible to cause damage to the edge of the wafer, such as chipping, cracks, etc. Figure 3The hidden cracks 12 formed at the edge of the wafer 10 are damaged. When the hidden cracks 12 are formed at the edge of the wafer after the front process of the wafer is completed, the stress of thinning will aggravate the degradation of the hidden cracks 12 at the edge of the wafer toward the front process area 13 of the product inside the wafer during the thinning process of the back of the wafer, resulting in chip damage in the front process area 13 of the product, affecting product reliability and reducing product yield.
[0031] Based on this, Figure 1 and Figure 2 As shown, Figure 2 FIG. 1 is a schematic diagram of a cross-sectional structure of a wafer with the back side facing upward. This embodiment provides a process method for thinning the back side of a wafer, and the process method includes:
[0032] S1, providing a wafer 10 that has completed the product front side process, and attaching a film to the front side of the wafer 10;
[0033] S2, performing annular laser invisible cutting on the edge of the wafer 10 from the back side of the wafer 10 to form an annular invisible isolation zone 11 at a preset depth inside the front edge of the wafer 10, and the invisible isolation zone 11 at least partially extends into the area corresponding to the product front process area 13 in the thickness direction of the wafer 10;
[0034] S3, thinning the back side of the wafer 10 so that the wafer 10 reaches a desired thickness;
[0035] S4, removing the front film of the wafer 10.
[0036] The process method for wafer back thinning of the present embodiment performs invisible laser cutting of the wafer edge from the back of the wafer after the wafer front is filmed and before the wafer back is thinned, so as to form an invisible ring-shaped isolation zone at a preset depth inside the wafer front edge, and the invisible isolation zone at least partially extends into the area corresponding to the product front process in the wafer thickness direction. The invisible isolation zone can block the transfer of stress during the wafer back thinning process, so that when the wafer edge is damaged during the product front process, the damage can be blocked from further expansion, that is, the damage at the wafer edge is blocked from further extending into the wafer interior (such as Figure 1 As shown in the figure, it can effectively reduce or even prevent the damage on the edge of the wafer from extending to the effective product, thus improving product reliability and product yield.
[0037] As an example, the material selection of the wafer 10 is based on the semiconductor device to be prepared, and any suitable semiconductor material can be selected, such as: a single layer structure of Si, Ge, SiGe, SiC, SiGeC, InAs, GaAs, InP, InGaAs or other III / V compound semiconductors; it can also be a multi-layer stacked structure composed of these semiconductor materials; it can also be silicon on insulator (SOI), stacked silicon on insulator (SSOI), stacked silicon germanium on insulator (S-SiGeOI), silicon germanium on insulator (SiGeOI) and germanium on insulator (GeOI). Generally, semiconductor devices are prepared on the semiconductor layer on the shallow surface of the front side of the wafer.
[0038] The material of the wafer front film is a sticky polymer material, such as HT140 material; the thickness of the film is selected according to actual needs, generally around 120μm to 160μm.
[0039] Since the laser's unique focusing, collimation and high energy characteristics can form defects inside the structure, in step S2, the invisible isolation zone 11 can be formed at a preset depth inside the wafer by laser cutting. Here, the "invisible" in the invisible isolation zone 11 refers to its formation inside the wafer. When forming the invisible isolation zone 11, the back side of the wafer is selected as the laser incident cutting surface to avoid damage to the effective product in the product front process area 13, resulting in a reduction in yield.
[0040] As a preferred example, a short pulse laser is used to perform annular laser invisible cutting on the edge of the wafer 10 to form the invisible isolation band 11. Short pulse lasers, such as picosecond and femtosecond lasers, can generate extremely high peak power and very short pulse width, and can accurately control the position of the invisible isolation band 11 in the wafer.
[0041] There is no excessive restriction on whether the invisible isolation belt 11 is a continuous invisible isolation belt. From its role, it can be seen that as long as the area where the damage on the edge of the wafer is located has the invisible isolation belt 11, it will have a blocking effect on the damage. Therefore, if it is known which areas on the edge of the wafer are prone to concentrated damage during the product front process, a continuous invisible isolation belt 11 can be formed in these areas with concentrated damage, and a discontinuous invisible isolation belt 11 can be formed in other areas. If it is not known which areas on the edge of the wafer are prone to damage during the product front process, the invisible isolation belt 11 can be set as a discontinuous invisible isolation belt 11 evenly arranged along the circumference, or the invisible isolation belt 11 can be set as a continuous invisible isolation belt 11 evenly arranged along the circumference. Relatively speaking, the continuous invisible isolation belt 11 has a better blocking effect on damage.
[0042] like Figure 1As shown, as a preferred example, the shape of the invisible isolation band 11 can be set to be the same as the shape of the wafer 10. For example, the general shape of the wafer 10 is circular, so the shape of the invisible isolation band 11 is also circular. Since the preparation of semiconductor devices on the front side of the wafer is generally arranged and prepared in accordance with the shape of the wafer to the maximum extent, the invisible isolation band 11 is set to the same circle as the wafer, which can minimize the damage to the effective products on the front side of the wafer. Furthermore, in the radial direction of the wafer 10, the distance L between the invisible isolation band 11 and the outer peripheral edge of the wafer 10 is 2.2mm~2.8mm, please refer to Figure 2 , the distance L refers to the distance between the outer side of the invisible isolation belt 11 and the outer peripheral edge of the wafer 10. The setting mode of the invisible isolation belt 11 with L=2.2mm-2.8mm can be as close to the inside of the wafer as possible in the radial direction while effectively ensuring that the effective products on the front of the wafer are damaged as little as possible, which can effectively improve the blocking effect of damage, and because it is close to the inside of the wafer in the radial direction, it is not easy to cause the edge of the wafer to fall off later.
[0043] It should be noted here that Figure 2 yes Figure 1 Schematic diagram of the cross-sectional structure at AA in the figure. For ease of understanding, Figure 2 It is not drawn to scale. Figure 2 The size of the invisible isolation zone 11 is correspondingly enlarged. Figure 2 As shown, as a preferred example, a portion of the thickness of the invisible isolation belt 11 extends into the area corresponding to the product front process area 13 in the thickness direction of the wafer 10, and another portion of the thickness extends into the area corresponding to the wafer thickness direction outside the product front process, such as Figure 2 The dotted line between the invisible isolation band 11 on the left side and the product front process area 13 divides the invisible isolation band 11 on the left side into a part that penetrates into the back side of the wafer 10 and a part of the area corresponding to the thickness of the wafer 10 where the product front process area 13 is located. This method can effectively block the damage from extending to the effective product on the front side of the wafer.
[0044] As an example, when the thickness of the wafer 10 is 700 μm to 750 μm, the preset depth of the invisible isolation band 11 inside the front edge of the wafer 10 is 10 μm to 300 μm, and the preset depth includes the thickness of the invisible isolation band 11 .
[0045] As an example, the width W of the invisible isolation belt is selected to be 3μm to 4μm. The width of the invisible isolation belt 11 should not be set too large or too small. If it is too large, it will cause loss of effective area of the wafer, and there may be a risk of wafer edge falling off during subsequent processes; if it is too small, the blocking effect on damage is poor. In addition, the thickness D of the invisible isolation belt is set according to actual needs, and the thickness D of the invisible isolation belt is selected based on different wafer thicknesses.
[0046] As an example, in step S3, a dual-axis process is used to thin the back side of the wafer 10.
[0047] In some application scenarios, power devices such as IGBT, VDMOS, SGT, etc. need to prepare a metal electrode coating on the back of the wafer, so after removing the front film of the wafer 10, the back of the wafer 10 is wet-grinded and a metal electrode coating is formed on the back of the wafer. The back of the wafer 10 is wet-grinded to remove the rough texture formed on the back of the wafer during the thinning process and reduce the contact resistance with the metal electrode coating formed subsequently; the metal electrode coating can be prepared by PVD process or evaporation process, and the material can be any material suitable for the electrode, such as aluminum, titanium, nickel and silver, etc.
[0048] In summary, the present invention provides a process method for thinning the back side of a wafer, after the wafer front side is filmed and before the wafer back side is thinned, the wafer edge is cut in an annular laser invisible manner from the back side of the wafer, so as to form an annular invisible isolation belt at a preset depth inside the front edge of the wafer, and the invisible isolation belt at least partially extends into the area corresponding to the product front process in the wafer thickness direction in the wafer thickness direction. The invisible isolation belt can block the transmission of stress during the thinning process of the back side of the wafer, so that when the edge of the wafer is damaged during the product front process, the further expansion of the damage can be blocked, that is, the damage of the edge of the wafer is blocked from further extending into the inside of the wafer, effectively reducing or even avoiding the damage of the edge of the wafer from extending to the effective product, thereby improving product reliability and product yield. Therefore, the present invention effectively overcomes various shortcomings in the prior art and has a high industrial utilization value.
[0049] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the art may modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by a person of ordinary skill in the art without departing from the spirit and technical concept disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A process for thinning the back side of a wafer, characterized in that: The process comprises: Providing wafers with completed product front-side processes and attaching a film to the front side of the wafers; Performing annular laser invisible cutting on the edge of the wafer from the back side of the wafer to form an annular invisible isolation zone at a preset depth inside the front edge of the wafer, and the invisible isolation zone at least partially extends in the thickness direction of the wafer to the area corresponding to the front process area of the product in the thickness direction of the wafer; Performing backside thinning on the wafer to make the wafer reach a desired thickness; The front side film of the wafer is removed.
2. The process for thinning the back side of a wafer according to claim 1, characterized in that: A short pulse laser is used to perform ring-shaped laser invisible cutting on the edge of the wafer.
3. The process for thinning the back side of a wafer according to claim 1, characterized in that: The invisible isolation belt is an annular continuous invisible isolation belt.
4. The process for thinning the back side of a wafer according to claim 1, characterized in that: The shape of the invisible isolation zone is the same as that of the wafer, both of which are circular.
5. The process for thinning the back side of a wafer according to claim 4, characterized in that: In the radial direction of the wafer, the distance between the invisible isolation zone and the outer peripheral edge of the wafer is 2.2 mm to 2.8 mm.
6. The process for wafer backside thinning according to claim 1, characterized in that: The wafer is back-thinned using a dual-axis process.
7. The process for thinning the back side of a wafer according to claim 1, characterized in that: After removing the film on the front side of the wafer, the method further includes the steps of wet grinding the back side of the wafer and forming a metal electrode coating on the back side of the wafer.
8. The process for wafer backside thinning according to claim 1, characterized in that: The thickness of the wafer is 700 μm to 750 μm, and the preset depth of the invisible isolation zone inside the front edge of the wafer is 10 μm to 300 μm.
9. The process for wafer backside thinning according to claim 1, characterized in that: The width of the invisible isolation zone is 3 μm to 4 μm.
10. The process for wafer backside thinning according to claim 1, characterized in that: Part of the thickness of the invisible isolation belt extends into the area corresponding to the product front process area in the wafer thickness direction, and the other part of the thickness extends into the area corresponding to the wafer thickness direction outside the product front process.
Citation Information
Cited By
Grinding control device and method for epitaxial wafer
CN122099978A