Zinc battery electrode modification method, prepared modified electrode and zinc battery
By forming an extremely thin solid-state electrolyte layer on the surface of the electrode of the zinc battery, the dendrites growth and resistance increase caused by SEI inhomogeneity in the zinc battery are solved, and uniform deposition of zinc ions and efficient mass transfer flux are achieved, which extends the Battery lifespan and Coulomb efficiency.
Patent Information
- Application Number
- CN202411041382.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-07-31
AI Technical Summary
The solid electrolyte interface (SEI) in existing zinc batteries is uneven, resulting in disordered deposition of zinc ions and dendritic growth, increasing resistance, reducing battery life and Coulomb efficiency.
By preparing the modified liquid, the cationic acceptor monomer, crosslinking agent and initiator are mixed, and the polymerization reaction is carried out to form an extremely thin solid-state electrolyte layer on the surface of the zinc electrode, which regulates the thickness and structure of SEI, inhibits the hydrogen evolution reaction and dendrites growth. .
The uniform deposition of zinc ions and efficient mass transfer flux are achieved, the cycle life and Coulomb efficiency of the battery are extended, the hydrogen evolution reaction and the generation of dendrites are inhibited, and the reversibility and stability of the battery are ensured.
Smart Images

Figure CN118983391A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of zinc batteries, and in particular to a method for modifying zinc battery electrodes and the prepared modified electrodes and zinc batteries. Background Art
[0002] During the operation of zinc-ion batteries, due to interfacial reactions, a solid electrolyte interface (SEI) with a thickness ranging from a few nanometers to tens of nanometers will inevitably form between the zinc anode and the electrolyte, which can stabilize the zinc anode in aqueous or non-aqueous electrolytes and improve the service life of zinc batteries. However, due to the inevitable problems of dendrite growth, corrosion and passivation during battery operation, the SEI is always uneven, which leads to a vicious cycle of disordered deposition and growth of zinc ions, aggravating the generation of dendrites. The dendrite tip easily pierces the SEI and continues to form a new SEI at the crack. This irreversible repeated damage and formation makes the SEI thicker and uneven, resulting in battery capacity loss, increased resistance, corrosion of the metal anode, poor cycle stability, and low Coulomb efficiency.
[0003] Based on this, various strategies have been proposed to promote the formation and optimization of SEI films, adjust the electrode / electrolyte interface to inhibit hydrogen evolution reaction and corrosion, reduce dendrite growth, and extend battery life and electrochemical stability window, such as adding organic / inorganic additives or artificial coatings. However, for the addition of organic / inorganic additives, the in-situ formation process of SEI during battery cycling is not controllable, so its structure, composition and thickness cannot be directly adjusted. In addition, the in-situ grown SEI layer is very sensitive to air, water vapor and carbon dioxide. When it leaves the original liquid electrolyte, the stable state will be broken, and the composition and thickness will undergo irreversible changes. Therefore, analysis and characterization need to be carried out under vacuum conditions, which places very high demands on the detection environment. Given the characterization limitations, there is currently no fixed conclusion on the structure of the in-situ SEI.
[0004] For the preparation of artificial SEI, the most common method is to prepare a protective layer on the negative electrode surface. However, when using a blade for scraping and coating, it is difficult to control the coating thickness and achieve a flat surface; if the spin coating method is used, the coating thickness can be controlled, but due to the effect of centrifugal force, the composition cannot be guaranteed to be in a uniform state; if electrospinning technology is used, the uniformity of the coating can only be displayed at the macro level, and the bonding between the protective layer and the substrate is still not tight. In addition, the thickness of the protective layer prepared by the above method is mostly in the micron level, which is difficult to control at the nanoscale, which will increase the interface resistance and further reduce the energy density. Summary of the invention
[0005] The technical problem to be solved by the present invention is how to prepare a very thin solid-state electrolyte layer in an electrode, clarify its structural composition, and reduce the interface resistance.
[0006] The present invention solves the above technical problems through the following technical means:
[0007] The first aspect of the present invention provides a method for modifying a zinc battery electrode, comprising the following steps:
[0008] (1) Preparation of a modified solution: dissolving a cation receptor monomer in a solvent, and adding a crosslinking agent and an initiator thereto to obtain a modified solution, wherein the cation receptor monomer is an amino derivative of an unsaturated ester;
[0009] (2) The modified liquid is coated on the electrode surface to carry out a polymerization reaction, and a modified electrode is obtained after the reaction.
[0010] Beneficial effects: The inventors artificially construct a quasi-solid electrolyte layer (SEI), clarify the composition of the SEI layer, and the quasi-solid electrolyte layer is closely connected with the electrode, and can improve the kinetic adsorption and mass transfer flux of zinc ions, effectively inhibit the hydrogen evolution reaction and the generation of zinc dendrites, and achieve the reversibility and ultra-long cycle life of the battery.
[0011] Preferably, the cation receptor monomer is dimethylaminoethyl methacrylate.
[0012] Preferably, the solvent is water; and the cross-linking agent is N,N-methylenebisacrylamide.
[0013] Preferably, the initiator is one of azobisisobutylimidazoline hydrochloride, potassium persulfate, and ammonium persulfate.
[0014] Preferably, the polymerization reaction is free radical polymerization.
[0015] Preferably, the mass concentration of the cation receptor monomer in the modified solution is 5-30 mg / ml.
[0016] Beneficial effects: The present invention regulates the thickness of the solid electrolyte layer (SEI) coated on the zinc negative electrode by regulating the mass concentration of the cation receptor monomer, so that the solid electrolyte layer is only tens of nanometers. By taking advantage of the differences in the binding force with zinc ions and the migration deposition rate caused by the different N atom concentrations at different thicknesses, the optimal overpotential for uniform deposition of zinc ions is determined, and a highly reversible aqueous zinc ion battery is constructed.
[0017] Preferably, the molar ratio of the cation receptor monomer: the cross-linking agent: the initiator is 1: 2% of the molar number of double bonds of the cation receptor monomer: 2% of the molar number of double bonds of the cation receptor monomer.
[0018] Preferably, the coating method adopts a drip coating-standing-back suction method.
[0019] The second aspect of the present invention provides a modified electrode prepared by the above zinc battery electrode modification method.
[0020] The third aspect of the present invention provides a zinc battery, comprising a modified electrode obtained by the above zinc battery electrode modification method.
[0021] The advantages of the present invention are:
[0022] The present invention artificially constructs a solid-state electrolyte layer (SEI) of the zinc electrode, and the thickness is only tens of nanometers, and the preparation process is simple. Different thicknesses of the solid-state electrolyte layer and different concentrations of N atoms lead to different binding forces for zinc ions, which in turn lead to different migration rates in the zinc ion deposition and dissolution process. The battery prepared at the optimal migration rate perfectly inhibits the hydrogen evolution reaction and the growth of zinc dendrites, and finally obtains a zinc battery prepared with a solid-state electrolyte layer that is extremely thin, has a clear structure, and is tightly combined with the electrode. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The zinc batteries prepared in Examples 1-4 and Comparative Example 1 were -2 and 1mAh cm -2 Long cycle performance under test conditions;
[0024] Figure 2 The zinc batteries prepared in Examples 1-4 and Comparative Example 1 were -2 and 10 mAh cm -2 Long cycle performance under test conditions;
[0025] Figure 3 The zinc batteries prepared in Example 2 and Comparative Example 1 were -2 and 1mAh cm -2 SEM image after 50 cycles under test conditions;
[0026] Figure 4 The zinc batteries prepared in Examples 5-8 and Comparative Example 2 were -2 Coulomb efficiency curve under test conditions;
[0027] Figure 5 is a FIB-SEM image characterizing the thickness of the quasi-solid electrolyte layer on the zinc electrode prepared in Example 2;
[0028] Bare Zn in the figure represents the unmodified zinc electrode. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0030] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.
[0031] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.
[0032] Example 1
[0033] This embodiment provides a zinc battery electrode modification method, a modified zinc electrode, and a zinc battery, which specifically include the following steps:
[0034] (1) Preparation of modified liquid:
[0035] 0.5 g of dimethylaminoethyl methacrylate was dissolved in 100 ml of water to obtain a 5 mg / ml dimethylaminoethyl methacrylate solution, and 10 mg of N,N-methylenebisacrylamide and 20 mg of azobisisobutylimidazoline hydrochloride were added thereto, and the mixture was stirred for 1 hour to obtain a modified solution.
[0036] (2) Preparation of modified zinc electrode:
[0037] The zinc foil disc used in this embodiment has a diameter of 12 mm and a thickness of 100 μm. The zinc foil disc is treated with 1M hydrochloric acid to remove surface oxides, and is placed in water for multiple ultrasonic cleanings, and then dried for use.
[0038] The modified liquid was applied on the treated surface of the zinc foil disc by drop coating, and allowed to stand for 15 minutes to allow the modified liquid to fully contact the zinc foil disc, and then the excess liquid was sucked back.
[0039] The zinc foil disc coated with 5 mg / ml modification liquid was placed in a closed device and nitrogen was blown for 15 minutes. Free radical polymerization was carried out at 65°C in a nitrogen atmosphere for 3 hours to obtain a modified zinc electrode loaded with poly(dimethylaminoethyl methacrylate) (Zn@PDM5).
[0040] (3) Preparation of zinc battery:
[0041] A CR2032 symmetrical battery was assembled using modified zinc electrodes as positive and negative electrodes, glass fiber as battery separator, and 2M zinc sulfate aqueous solution as electrolyte.
[0042] Example 2
[0043] This embodiment provides a zinc battery electrode modification method, a modified zinc electrode and a zinc battery. This embodiment is different from Embodiment 1 in that: Step (1) is as follows:
[0044] (1) Preparation of modified liquid:
[0045] 1.0 g of dimethylaminoethyl methacrylate was dissolved in 100 ml of water to obtain a 10 mg / ml dimethylaminoethyl methacrylate solution, and 20 mg of N,N-methylenebisacrylamide and 40 mg of azobisisobutylimidazoline hydrochloride were added thereto, and the mixture was stirred for 1 hour to obtain a modified solution.
[0046] Steps (2) and (3) are exactly the same as in the example to obtain a modified zinc electrode (Zn@PDM 10 ).
[0047] Example 3
[0048] This embodiment provides a zinc battery electrode modification method, a modified zinc electrode and a zinc battery. This embodiment is different from Embodiment 1 in that: Step (1) is as follows:
[0049] (1) Preparation of modified liquid:
[0050] 2.0 g of dimethylaminoethyl methacrylate was dissolved in 100 ml of water to obtain a 20 mg / ml dimethylaminoethyl methacrylate solution, and 40 mg of N,N-methylenebisacrylamide and 80 mg of azobisisobutylimidazoline hydrochloride were added thereto, and the mixture was stirred for 1 hour to obtain a modified solution.
[0051] Steps (2) and (3) are exactly the same as in the example to obtain a modified zinc electrode (Zn@PDM 20 ).
[0052] Example 4
[0053] This embodiment provides a zinc battery electrode modification method, a modified zinc electrode and a zinc battery. This embodiment is different from Embodiment 1 in that: Step (1) is as follows:
[0054] (1) Preparation of modified liquid:
[0055] 3.0 g of dimethylaminoethyl methacrylate was dissolved in 100 ml of water to obtain a 30 mg / ml dimethylaminoethyl methacrylate solution, to which 60 mg of N,N-methylenebisacrylamide and 120 mg of azobisisobutylimidazoline hydrochloride were added, and the mixture was stirred for 1 hour to obtain a modified solution.
[0056] Steps (2) and (3) are exactly the same as in Example 1. The modified zinc electrode (Zn@PDM 30 ).
[0057] Example 5
[0058] This embodiment provides a zinc battery electrode modification method, a modified zinc electrode, a modified copper electrode and a zinc-copper half-cell, which specifically include the following steps:
[0059] (1) Preparation of modified liquid:
[0060] 0.5 g of dimethylaminoethyl methacrylate was dissolved in 100 ml of water to obtain a 5 mg / ml dimethylaminoethyl methacrylate solution, and 10 mg of N,N-methylenebisacrylamide and 20 mg of azobisisobutylimidazoline hydrochloride were added thereto, and the mixture was stirred for 1 hour to obtain a modified solution.
[0061] (2) Preparation of modified electrodes:
[0062] The zinc foil disc used in this embodiment has a diameter of 12 mm and a thickness of 100 μm. The zinc foil disc is treated with 1M hydrochloric acid to remove surface oxides, and is placed in water for multiple ultrasonic cleanings, and then dried for use.
[0063] The copper foil disc used in this embodiment has a diameter of 12 mm and a thickness of 20 μm. The copper foil disc is polished with sandpaper to remove surface oxides, and is placed in ethanol for multiple ultrasonic cleaning, and then dried for use.
[0064] The modified liquid was applied to the treated surfaces of the zinc foil and copper foil discs by drop coating, and allowed to stand for 15 minutes to allow the modified liquid to fully contact the zinc foil and copper foil discs, and then the excess liquid was sucked back.
[0065] The zinc foil and copper foil discs coated with 5 mg / ml modification liquid were placed in a closed device and blown with nitrogen for 15 minutes. Free radical polymerization was carried out at 65°C in a nitrogen atmosphere for 3 hours to obtain modified zinc electrodes (Zn@PDM5) and modified copper electrodes (Cu@PDM5) loaded with poly(dimethylaminoethyl methacrylate).
[0066] (3) Preparation of zinc-copper half-cell:
[0067] A CR2032 type Zn / Cu half-cell was assembled using the modified zinc electrode as the negative electrode, the modified copper electrode as the positive electrode, glass fiber as the battery separator, and a 2M zinc sulfate aqueous solution as the electrolyte.
[0068] Example 6
[0069] This embodiment provides a zinc battery electrode modification method, a modified zinc electrode, a modified copper electrode and a zinc-copper half-cell, which specifically include the following steps:
[0070] The difference between this embodiment and embodiment 5 is that step (1) is as follows:
[0071] (1) Preparation of modified liquid:
[0072] 1.0 g of dimethylaminoethyl methacrylate was dissolved in 100 ml of water to obtain a 10 mg / ml dimethylaminoethyl methacrylate solution, and 20 mg of N,N-methylenebisacrylamide and 40 mg of azobisisobutylimidazoline hydrochloride were added thereto, and the mixture was stirred for 1 hour to obtain a modified solution.
[0073] Steps (2) and (3) are exactly the same as in the example to obtain a modified zinc electrode (Zn@PDM 10 ) and modified copper electrode (Cu@PDM 10 ).
[0074] Example 7
[0075] This embodiment provides a zinc battery electrode modification method, a modified zinc electrode, a modified copper electrode and a zinc-copper half-cell, which specifically include the following steps:
[0076] The difference between this embodiment and embodiment 5 is that step (1) is as follows:
[0077] (1) Preparation of modified liquid:
[0078] 2.0 g of dimethylaminoethyl methacrylate was dissolved in 100 ml of water to obtain a 20 mg / ml dimethylaminoethyl methacrylate solution, and 40 mg of N,N-methylenebisacrylamide and 80 mg of azobisisobutylimidazoline hydrochloride were added thereto, and the mixture was stirred for 1 hour to obtain a modified solution.
[0079] Steps (2) and (3) are exactly the same as in the example to obtain a modified zinc electrode (Zn@PDM 20 ) and modified copper electrode (Cu@PDM 20 ).
[0080] Example 8
[0081] This embodiment provides a zinc battery electrode modification method, a modified zinc electrode, a modified copper electrode and a zinc-copper half-cell, which specifically include the following steps:
[0082] The difference between this embodiment and embodiment 5 is that step (1) is as follows:
[0083] (1) Preparation of modified liquid:
[0084] 3.0 g of dimethylaminoethyl methacrylate was dissolved in 100 ml of water to obtain a 30 mg / ml dimethylaminoethyl methacrylate solution, to which 60 mg of N,N-methylenebisacrylamide and 120 mg of azobisisobutylimidazoline hydrochloride were added, and the mixture was stirred for 1 hour to obtain a modified solution.
[0085] Steps (2) and (3) are exactly the same as in the example to obtain a modified zinc electrode (Zn@PDM 30 ) and modified copper electrode (Cu@PDM 30 ).
[0086] Example 9
[0087] This embodiment provides a zinc battery electrode modification method, a modified zinc electrode and a zinc battery. This embodiment is different from Embodiment 1 in that: Step (1) is as follows:
[0088] (1) Preparation of modified liquid:
[0089] 0.5 g of dimethylaminoethyl methacrylate was dissolved in 100 ml of water to obtain a 5 mg / ml dimethylaminoethyl methacrylate solution, to which 10 mg of N,N-methylenebisacrylamide and 17 mg of potassium persulfate were added, and the mixture was stirred for 1 hour to obtain a modified solution.
[0090] Steps (2) and (3) are exactly the same as in the example to obtain a modified zinc electrode (Zn@PDM5).
[0091] Example 10
[0092] This embodiment provides a zinc battery electrode modification method, a modified zinc electrode and a zinc battery. This embodiment is different from Embodiment 1 in that: Step (1) is as follows:
[0093] (1) Preparation of modified liquid:
[0094] 0.5 g of dimethylaminoethyl methacrylate was dissolved in 100 ml of water to obtain a 5 mg / ml dimethylaminoethyl methacrylate solution, to which 10 mg of N,N-methylenebisacrylamide and 15 mg of ammonium persulfate were added, and the mixture was stirred for 1 hour to obtain a modified solution.
[0095] Steps (2) and (3) are exactly the same as in the example to obtain a modified zinc electrode (Zn@PDM5).
[0096] Embodiment 11
[0097] This embodiment provides a zinc battery electrode modification method, a modified zinc electrode and a zinc battery. This embodiment is different from Embodiment 1 in that: Step (1) is as follows:
[0098] (1) Preparation of modified liquid:
[0099] 2 g of dimethylaminoethyl methacrylate was dissolved in 100 ml of water to obtain a 20 mg / ml dimethylaminoethyl methacrylate solution, to which 40 mg of N,N-methylenebisacrylamide and 68 mg of potassium persulfate were added, and the mixture was stirred for 1 hour to obtain a modified solution.
[0100] Steps (2) and (3) are exactly the same as in the example to obtain a modified zinc electrode (Zn@PDM 20 ).
[0101] Example 12
[0102] This embodiment provides a zinc battery electrode modification method, a modified zinc electrode and a zinc battery. This embodiment is different from Embodiment 1 in that: Step (1) is as follows:
[0103] (1) Preparation of modified liquid:
[0104] 3 g of dimethylaminoethyl methacrylate was dissolved in 100 ml of water to obtain a 30 mg / ml dimethylaminoethyl methacrylate solution, to which 60 mg of N,N-methylenebisacrylamide and 102 mg of potassium persulfate were added, and the mixture was stirred for 1 hour to obtain a modified solution.
[0105] Steps (2) and (3) are exactly the same as in the example to obtain a modified zinc electrode (Zn@PDM 30 ).
[0106] Comparative Example 1
[0107] A zinc foil disc with a diameter of 12 mm and a thickness of 100 μm was treated with 1M hydrochloric acid to remove surface oxides, and then placed in water for multiple ultrasonic cleanings, and then dried for use. Then the zinc foil disc was used as the positive and negative electrodes, the glass fiber was used as the battery separator, and the 2M zinc sulfate aqueous solution was used as the electrolyte to assemble a CR2032 type symmetrical battery.
[0108] Comparative Example 2
[0109] A zinc foil disc with a diameter of 12 mm and a thickness of 20 μm was treated with 1M hydrochloric acid to remove the surface oxide, and then placed in water for multiple ultrasonic cleaning, and then dried for use. A copper foil disc with a diameter of 12 mm and a thickness of 20 μm was polished with sandpaper to remove the surface oxide, and then placed in ethanol for multiple ultrasonic cleaning, and then dried for use. A CR2032 type Zn / Cu half-cell was assembled using a zinc foil disc as the negative electrode, a copper foil disc as the positive electrode, glass fiber as the battery separator, and a 2M zinc sulfate aqueous solution as the electrolyte.
[0110] from Figure 1 and Figure 2 It can be seen that the symmetrical cells assembled with modified zinc electrodes in Examples 1-4 all have cycle performances that are better than the symmetrical cell assembled with unmodified zinc electrodes in Comparative Example 1. Among them, the polymethacrylic acid film prepared by coating 10 mg / ml of the modified solution has the best protective effect on the zinc negative electrode, with a cycle performance of 1 mA cm -2 The current density and 1 mAh cm -2 The cycle life is more than 1600 h at an area density of 10 mA cm -2 The current density and 10 mAh cm -2 The cycle life is more than 1000h at an area density of .
[0111] Figure 3 The SEM images show that the PDM coated 10 The surface of the zinc foil after the layer is smoother and flatter. In contrast, the surface of the bare zinc foil has a large number of zinc dendrites with disordered deposition direction, which further grows into sharp flakes, seriously affecting the performance and safety of the battery. 10 No obvious dendrites were observed on the electrode surface because the appropriate overpotential led to a more uniform and denser Zn deposition, thus suppressing the generation of Zn dendrites.
[0112] Figure 4 The Coulomb efficiency diagram shows that at a current density of 1 mA cm -2 In the case of , the batteries prepared by the modified solution system are better than the bare zinc electrode, and the cycle times are more than 4 times. 10 The electrode is optimal. 10 The battery assembled from the electrodes provides a long-term stable Coulombic efficiency of 99.6% and has a cycle life of up to 1700 times, fully demonstrating that this system has good zinc plating / stripping reversibility.
[0113] Figure 5 The FIB-SEM image clearly characterizes the thickness of the quasi-solid electrolyte layer. It can be seen from the image that a thin layer is visible between the Zn and Pt / C protective layers, and the thickness of the layer is about 60nm, indicating that an extremely thin quasi-solid electrolyte layer of only tens of nanometers has been successfully prepared on the zinc electrode.
[0114] From the comparison between the embodiment and the comparative example, it can be concluded that the good cycle performance, surface morphology and coulombic efficiency prove that the solid-state electrolyte layer helps N atoms on the negative electrode surface to regulate the migration flux and deposition direction of zinc ions at the interface, effectively inhibits the generation of zinc dendrites and by-products, and prolongs the service life of the battery.
[0115] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A zinc battery electrode modification method, characterized in that: The following steps are involved: (1) Preparation of a modified solution: dissolving a cation receptor monomer in a solvent, and adding a crosslinking agent and an initiator thereto to obtain a modified solution, wherein the cation receptor monomer is an amino derivative of an unsaturated ester; (2) The modified liquid is coated on the electrode surface to carry out a polymerization reaction, and a modified electrode is obtained after the reaction.
2. The zinc battery electrode modification method according to claim 1, characterized in that: The cation receptor monomer is dimethylaminoethyl methacrylate.
3. The zinc battery electrode modification method according to claim 1, characterized in that: The mass concentration of the cation receptor monomer in the modified solution is 5-30 mg / ml.
4. The zinc battery electrode modification method according to claim 1, characterized in that: The solvent is water; the cross-linking agent is N,N-methylenebisacrylamide.
5. The zinc battery electrode modification method according to claim 1, characterized in that: The initiator is one of azobisisobutylimidazoline hydrochloride, potassium persulfate and ammonium persulfate.
6. The zinc battery electrode modification method according to claim 1, characterized in that: The polymerization reaction is free radical polymerization.
7. The zinc battery electrode modification method according to claim 1, characterized in that: The molar ratio of the cation receptor monomer: the cross-linking agent: the initiator is 1: 2% of the molar number of double bonds of the cation receptor monomer: 2% of the molar number of double bonds of the cation receptor monomer.
8. The zinc battery electrode modification method according to claim 1, characterized in that: The coating method adopts a drop coating-standing-back sucking method.
9. A modified electrode prepared by the zinc battery electrode modification method according to any one of claims 1 to 8.
10. A zinc battery, characterized in that: The modified electrode is prepared by the zinc battery electrode modification method as described in any one of claims 1 to 8.
Citation Information
Patent Citations
Composite polymer electrolyte and application thereof in battery cathode protection
CN105789695A
Zinc metal negative electrode with amino silane polymer protective layer and preparation method of zinc metal negative electrode
CN114843431A
Zinc metal negative electrode and zinc battery
CN116314566A
Apparatus for measuring thickness and collecting battery gas of bettery cell
KR102654390B1