Sodium-ion battery positive electrode material and preparation method thereof, positive plate, sodium-ion battery and electric equipment
By using sodium, nickel, titanium, manganese and boron sources in the positive electrode material of sodium ion battery, the NawNixTiyMnzB1-x-y-zO2 material with high air stability and low residual alkali was generated, and the layered structure was solved. The problem of poor storage properties of transition metal oxides and excessive residual alkali on the surface achieves a sodium ion battery with high capacity and excellent circulation performance.
Patent Information
- Application Number
- CN202411040505.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-19
AI Technical Summary
The layered structure transition metal oxide has poor storage properties in the air, excessive residual alkali on the surface leads to gelation of the positive electrode slurry, increases the internal resistance of the battery, and poor capacity, circulation and rate performance.
Using the preparation method of sodium ion battery positive electrode material, by mixing and sintering sodium, nickel, titanium, manganese and boron sources, NawNixTiyMnzB1-x-y-zO2 material with high air stability and low residual alkali content, and The material surface forms a cladding layer of NaBO2 and CaO to slow down side reactions and improve circulation performance.
It realizes the high capacity, excellent cycle performance and rate performance of sodium ion batteries, and the preparation method is simple and low cost, which is suitable for large-scale production.
Smart Images

Figure CN118983432A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion battery positive electrode materials, and in particular to a sodium ion battery positive electrode material and a preparation method thereof, a positive electrode sheet, a sodium ion battery and an electrical device. Background Art
[0002] Sodium-ion batteries are expected to be first used in large-scale energy storage devices and low-speed transportation due to their high safety, abundant raw material sources and low cost. Among them, layered metal oxides have a high specific capacity, making them the most promising sodium-ion battery positive electrode material for commercial production.
[0003] However, layered transition metal oxides have poor storage properties in the air and have excess residual alkali on their surface, which usually causes gelation of the positive electrode slurry. Serious interfacial side reactions are likely to occur in the electrolyte, leading to an increase in the internal resistance of the battery, resulting in poor capacity, cycle performance and rate performance.
[0004] In view of this, the present invention is proposed. Summary of the invention
[0005] The first object of the present invention is to provide a sodium ion battery positive electrode material with good air stability and low residual alkali content. The battery prepared therefrom has high capacity and good cycle performance and rate performance.
[0006] The second object of the present invention is to provide a method for preparing a positive electrode material for a sodium ion battery, which has the advantages of simple operation, short process, low production cost and easy large-scale production.
[0007] The third object of the present invention is to provide a positive electrode sheet.
[0008] A fourth object of the present invention is to provide a sodium ion battery.
[0009] A fifth object of the present invention is to provide an electrical device.
[0010] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0011] The present invention first provides a sodium ion battery positive electrode material, the general formula of the sodium ion battery positive electrode material is Na w Ni x Ti y Mn z B 1-x-y-z O2; among them, 0.6≤w≤0.9, 0.2≤x≤0.5, 0.1≤y≤0.2, 0.4≤z≤0.6, 0.05≤1-xyz≤0.25.
[0012] Preferably, at a temperature of 20 to 25° C., the pH of the aqueous solution with a mass fraction of 32.5% to 33.5% of the sodium ion battery positive electrode material is 12.2 to 12.75.
[0013] Preferably, the median particle size of the sodium ion battery positive electrode material is 3 to 15 μm.
[0014] The present invention further provides a method for preparing the positive electrode material of a sodium ion battery, comprising the following steps: mixing a sodium source, a nickel source, a titanium source, a manganese source and a boron source and then sintering the mixture.
[0015] Preferably, the boron source includes at least one of calcium boride, silicon boride, chromium boride, boron nitride and boron bromide.
[0016] Preferably, the sintering temperature is 900-1200° C., and the holding time is 15-20 hours.
[0017] The present invention further provides a positive electrode sheet, comprising the positive electrode material for a sodium ion battery.
[0018] Preferably, the positive electrode sheet also includes chloride.
[0019] Wherein, the mass of the chloride is 0.5% to 1% of the mass of the sodium ion battery positive electrode material, and / or the chloride includes at least one of potassium chloride, calcium chloride, barium chloride, ferric chloride, ferrous chloride, cupric chloride, and aluminum chloride.
[0020] The present invention further provides a sodium ion battery, comprising the positive electrode sheet.
[0021] The present invention also provides an electrical device, comprising the sodium ion battery.
[0022] Compared with the prior art, the present invention has the following beneficial effects:
[0023] The sodium ion battery positive electrode material provided by the invention has good air stability and low residual alkali content; the battery prepared therefrom has high capacity and good cycle performance and rate performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0025] Figure 1 This is a SEM image of the sodium ion battery positive electrode material prepared in Example 1 provided by the present invention;
[0026] Figure 2 The XRD diagram of the sodium ion battery positive electrode material prepared in Example 1 provided by the present invention;
[0027] Figure 3 A comparison diagram of the first charge and discharge curves of batteries assembled with the sodium ion battery positive electrode materials of Examples 1 to 3 provided by the present invention;
[0028] Figure 4 A comparison chart of 200 cycle curves of batteries assembled with the sodium ion battery positive electrode materials of Examples 1 to 3 provided by the present invention;
[0029] Figure 5 A comparison diagram of the first charge and discharge curves of batteries assembled with the sodium ion battery positive electrode materials of Comparative Examples 1 to 4 provided by the present invention;
[0030] Figure 6 This is a comparison chart of the 200-cycle curves of batteries assembled with the sodium ion battery positive electrode materials of Comparative Examples 1 to 4 provided by the present invention. DETAILED DESCRIPTION
[0031] The technical scheme of the present invention will be clearly and completely described below in conjunction with the accompanying drawings and specific embodiments, but it will be understood by those skilled in the art that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified in the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0032] If there is no special explanation, in the present invention, "the first aspect", "the second aspect", "the third aspect", "the fourth aspect", etc. are only used for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "the first", "the second", "the third", "the fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.
[0033] If there is no special explanation, the "include" and "comprising" mentioned in the present invention represent open-ended or closed-ended expressions. For example, the "include" and "comprising" may represent that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0034] If there is no special explanation, in the present invention, "one or more" or "at least one" refers to any one, any two or more of the listed items. Among them, "several" refers to any two or more of the listed items.
[0035] In the first aspect, the present invention provides a boride-doped low-nickel, high-capacity, high-air-stable sodium ion battery positive electrode material, the general formula of the sodium ion battery positive electrode material is Na w Ni x Ti y Mn z B 1-x-y-z O2.
[0036] Among them, 0.6≤w≤0.9, 0.2≤x≤0.5, 0.1≤y≤0.2, 0.4≤z≤0.6, 0.05≤1-xyz≤0.25.
[0037] Wherein, w includes but is not limited to any one of 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9 or a range of values between any two of them; x includes but is not limited to any one of 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5 or a range of values between any two of them; y includes but is not limited to any one of 0.1, 0.12, 0.13, 0.15, 0.16, 0.18, 0.2 or a range of values between any two of them; z includes but is not limited to any one of 0.4, 0.45, 0.5, 0.55, 0.6 or a range of values between any two of them; the value of 1-xyz includes but is not limited to any one of 0.05, 0.08, 0.1, 0.12, 0.14, 0.15, 0.2, 0.25 or a range of values between any two of them.
[0038] In some specific embodiments, the B element in the sodium ion battery positive electrode material is derived from a boron source, that is, a boron-containing substance, and the boron source includes at least one of calcium boride, silicon boride, chromium boride, boron nitride and boron bromide.
[0039] The sodium ion battery positive electrode material provided by the present invention has good air stability, low residual alkali content, high charge and discharge specific capacity, excellent rate performance and air stability, and can be used as a sodium battery material with high specific capacity, high rate and high air stability.
[0040] In the process of preparing positive electrode materials for sodium ion batteries, the sodium source decomposes into Na2O and CO2 under high temperature conditions, and the boron-containing substance reacts with the decomposition product Na2O to generate NaBO2 and high-valent oxidation by-products (for example, if the boron source is CaB6, the by-product is CaO).
[0041] Taking CaB6 as the boron source, the reaction formula is as follows:
[0042] Na2CO3→Na2O+CO2↑;
[0043] 3Na2O+CaB6+5O2→6NaBO2+CaO;
[0044] 2CaB 6+ 12H2O+13O2→12H2BO3+2CaO.
[0045] The generated NaBO2 has a good sodium replenishing effect and can improve the later long cycle life of the battery; during the cooling process, a coating layer with the main components of NaBO2 and CaO (high-valent oxidation by-product) is formed on the surface of the material, which effectively improves the cycle performance and air stability of the positive electrode material, ensures the close combination and complete coverage of effective by-products, and slows down the side reactions between the positive electrode material and the electrolyte.
[0046] In addition, as a superconductor material, boron-containing substances have high chemical stability, high thermal conductivity and high electrical conductivity. High electrical conductivity can enhance the electrical conductivity of the material, and high chemical stability plays a physical isolation role to avoid corrosion by the electrolyte. The wettability of the reaction of boron-containing substances with layered oxides can penetrate into the primary particles, which can ensure the close bonding of the layered oxides, thereby helping to improve the structural stability of the positive electrode material. Boron-containing substances are also oxygen-affinity and can react slightly with the oxygen on the surface of the positive electrode material particles to form a bond, effectively stabilizing the oxygen on the surface of the positive electrode material and inhibiting the precipitation of lattice oxygen.
[0047] In summary, the boron-containing coating material is evenly dispersed on the surface of the positive electrode material. After reacting with the moisture in the material to generate boric acid, it can reduce the hygroscopicity (water absorption) of the material and neutralize the alkalinity of the material. At the same time, it improves the electronic conductivity of the positive electrode material, and can also inhibit side reactions with the electrolyte and reduce gas production. Among them, the boron element can work synergistically with Ni and Mn to make the material have a higher reversible specific capacity, and the addition of Ti improves its stability. The combination of these elements can finally obtain a sodium ion battery positive electrode material with high capacity and stable cycle performance.
[0048] In some specific embodiments, at an ambient temperature of 20 to 25° C., the pH of an aqueous solution containing 32.5% to 33.5% of the sodium ion battery cathode material is 12.2 to 12.75, wherein the pH includes but is not limited to any point value of 12.2, 12.25, 12.3, 12.4, 12.5, 12.55, 12.6, and 12.75 or a range value between any two of them. It can be seen that the alkalinity of the sodium ion battery cathode material is relatively low.
[0049] In some specific embodiments, the median particle size D of the sodium ion battery positive electrode material is 50It is 3 to 15μm, including but not limited to any point value of 3μm, 4μm, 5μm, 6μm, 7μm, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, and 15μm, or a range value between any two of them.
[0050] In some specific embodiments, the positive electrode material of the sodium ion battery is a mixed layered oxide of P2 and O3.
[0051] In a second aspect, the present invention provides a method for preparing the above-mentioned sodium ion battery positive electrode material, comprising the following steps: mixing a sodium source, a nickel source, a titanium source, a manganese source and a boron source evenly, sintering, and cooling to obtain a sodium ion battery positive electrode material.
[0052] The preparation method has a simple process, readily available and low-priced raw materials, and has a high degree of practicability.
[0053] Moreover, the sodium ion battery assembled using the positive electrode material prepared by the above method has high specific capacity and excellent cycle performance.
[0054] Specifically, during the preparation of the positive electrode material for sodium ion batteries, at a high temperature between 800-900°C, the sodium source decomposes into Na2O and CO2, and the boron-containing substance begins to react with the decomposition product sodium oxide above 900°C to generate NaBO2 and a high-valent oxidation byproduct (if the boron source is CaB6, the byproduct is CaO).
[0055] Taking CaB6 as the boron source, the reaction formula is as follows:
[0056] Taking CaB6 as the boron source, the reaction formula is as follows:
[0057] Na2CO3→Na2O+CO2↑;
[0058] 3Na2O+CaB6+5O2→6NaBO2+CaO;
[0059] 2CaB 6+ 12H2O+13O2→12H2BO3+2CaO.
[0060] The generated NaBO2 has a good sodium supplementation effect and improves the battery's later long cycle life. During the gradual cooling of the material, a coating layer of NaBO2 and CaO (high-valent oxidation byproduct) is formed on the surface of the material. The cycle performance and air stability of the positive electrode material are effectively improved. The tight combination and complete coverage of the effective byproducts are ensured, slowing down the side reactions between the positive electrode material and the electrolyte.
[0061] In some specific embodiments, the boron source includes at least one of calcium boride, silicon boride, chromium boride, boron nitride and boron bromide. The present invention does not use hazardous chemicals such as boron hydride compounds, and is safer.
[0062] In some specific embodiments, the sintering temperature is 900-1200°C, including but not limited to any point value of 900°C, 950°C, 1000°C, 1050°C, 1100°C, 1150°C, 1200°C or a range between any two of them.
[0063] In some specific embodiments, the sintering holding time is 15 to 20 hours, including but not limited to any one of 15 hours, 16 hours, 17 hours, 18 hours, 19 hours, and 20 hours, or a range between any two of them.
[0064] In some specific embodiments, the mixing method includes grinding, such as ball milling. Preferably, the grinding time is 5 to 15 hours.
[0065] In some specific embodiments, the sintering is performed in an oxygen-containing atmosphere, such as an air atmosphere or an oxygen atmosphere.
[0066] In some specific embodiments, the sintering is performed in a muffle furnace, for example, the raw materials are placed in a corundum crucible and transferred to a muffle furnace for sintering.
[0067] In some specific implementations, the heating rate of the sintering is 2-5° C. / min.
[0068] In some specific embodiments, by controlling the content of the sodium source and the sintering temperature, the sodium ion battery positive electrode material is a P2 and O3 mixed layered oxide.
[0069] In a third aspect, the present invention provides a positive electrode sheet comprising the above-mentioned sodium ion battery positive electrode material.
[0070] In some specific implementations, the positive electrode sheet also includes chloride.
[0071] The present invention can solve the gelation problem of positive electrode slurry and the problem of difficulty in first or mid-charge by adding chloride to absorb moisture in positive electrode materials, conductive agents and binders, thereby further improving the performance of the battery.
[0072] In some specific embodiments, the mass of the chloride is 0.5% to 1% of the mass of the sodium ion battery positive electrode material, including but not limited to any one of 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1% or a range between any two of them.
[0073] In some specific embodiments, the chloride includes at least one of potassium chloride, calcium chloride, barium chloride, ferric chloride, ferrous chloride, cupric chloride, and aluminum chloride.
[0074] In a fourth aspect, the present invention provides a sodium ion battery comprising the above-mentioned positive electrode sheet.
[0075] The sodium ion battery provided by the present invention can be used as a new type of high energy density energy storage battery which is easy to prepare and convenient to store, and has a good application prospect.
[0076] Optionally, the positive electrode sheet further includes a conductive agent and / or a binder.
[0077] The sodium ion battery provided by the present invention can be applied to various fields, such as the field of transportation, the field of electronic products, the field of aerospace, the field of medical treatment, and the field of energy storage, but is not limited thereto.
[0078] In a fifth aspect, the present invention provides an electrical device comprising the above-mentioned sodium ion battery.
[0079] Among them, electrical equipment includes any equipment or devices that use the above-mentioned sodium ion batteries, such as electric vehicles, electric motorcycles, electric bicycles, electric tools, starting power supplies, energy storage equipment, electronic products, office equipment, etc., but not limited to these.
[0080] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.
[0081] Example 1
[0082] The method for preparing the positive electrode material of a sodium ion battery provided in this embodiment comprises the following steps: 0.83 Ni 0.3 Ti 0.3 Mn 0.3 B 0.1 O2 Weigh the corresponding proportions of the raw materials, where the sodium source is sodium carbonate, the nickel source is nickel oxide, the titanium source is titanium dioxide, the manganese source is manganese tetraoxide, and the boron source is calcium boride. The raw materials are mixed by ball milling for 5 hours. The median particle size of the ground mixture is 13μm. The mixture is then transferred to a crucible and sintered in a box-type muffle furnace at 1200℃ for 15 hours. After cooling, it is crushed in a mortar to obtain a sodium ion battery positive electrode material with a median particle size of 8μm.
[0083] At a temperature of 25° C., the pH value of the aqueous solution with a mass fraction of 33% of the sodium ion battery positive electrode material prepared in this embodiment is 12.47.
[0084] like Figure 1The SEM image of the sodium ion battery positive electrode material prepared in Example 1 is shown. Figure 2 Shown is the XRD pattern of the sodium ion battery positive electrode material prepared in Example 1.
[0085] Example 2
[0086] The preparation method of the sodium ion battery positive electrode material provided in this embodiment is basically the same as that in Example 1, except that calcium boride is replaced by silicon boride in an equal molar amount based on the boron element.
[0087] At a temperature of 25° C., the pH value of the aqueous solution with a mass fraction of 33% of the sodium ion battery positive electrode material prepared in this embodiment is 12.45.
[0088] Example 3
[0089] The preparation method of the sodium ion battery positive electrode material provided in this embodiment is basically the same as that in Example 1, except that calcium boride is replaced by chromium boride in an equal molar amount based on the boron element.
[0090] At a temperature of 25° C., the pH value of the aqueous solution with a mass fraction of 33% of the sodium ion battery positive electrode material prepared in this embodiment is 12.51.
[0091] Example 4
[0092] The preparation method of the sodium ion battery positive electrode material provided in this embodiment is basically the same as that in Example 1, except that calcium boride is replaced by boron nitride in an equal molar amount based on the boron element.
[0093] At a temperature of 25° C., the pH value of the aqueous solution of the sodium ion battery positive electrode material prepared in this embodiment with a mass fraction of 33% was 12.39.
[0094] Example 5
[0095] The preparation method of the sodium ion battery positive electrode material provided in this embodiment is basically the same as that in Example 1, except that calcium boride is replaced by boron bromide in an equimolar amount based on the boron element.
[0096] At a temperature of 25° C., the pH value of the aqueous solution of the sodium ion battery positive electrode material prepared in this embodiment with a mass fraction of 33% was 12.41.
[0097] Example 6
[0098] The preparation method of the sodium ion battery positive electrode material provided in this embodiment is basically the same as that in Example 1, except that the material is sintered at 1100° C. for 20 h.
[0099] At a temperature of 25° C., the pH value of the aqueous solution with a mass fraction of 33% of the sodium ion battery positive electrode material prepared in this embodiment is 12.38.
[0100] Example 7
[0101] The preparation method of the sodium ion battery positive electrode material provided in this embodiment is basically the same as that in Example 1, except that 0.83 Ni 0.3 Ti 0.25 Mn 0.3 B 0.15 O2 weighs the raw materials in corresponding proportions.
[0102] At a temperature of 25° C., the pH value of the aqueous solution with a mass fraction of 33% of the sodium ion battery positive electrode material prepared in this embodiment is 12.44.
[0103] Example 8
[0104] The preparation method of the sodium ion battery positive electrode material provided in this embodiment is basically the same as that in Example 1, except that 0.83 Ni 0.3 Ti 0.15 Mn 0.3 B 0.25 O2 weighs the raw materials in corresponding proportions.
[0105] At a temperature of 25° C., the pH value of the aqueous solution with a mass fraction of 33% of the sodium ion battery positive electrode material prepared in this embodiment is 12.42.
[0106] Example 9-Example 16
[0107] Example 9, Example 10, Example 11, Example 12, Example 13, Example 14, Example 15, and Example 16 respectively use the sodium ion battery positive electrode materials obtained in Example 1, Example 2, Example 3, Example 4, Example 5, Example 6, Example 7, and Example 8 as positive electrode active materials, and prepare positive electrode sheets according to the following method: Weigh each raw material in a ratio of 8:10:10 (mass ratio of positive electrode active material: conductive agent (Super-P): binder (PVDF)), mix them evenly, then add solvent NMP (N-methylpyrrolidone) thereto, mix evenly to obtain positive electrode slurry, apply it on aluminum foil, and then place it in a vacuum drying oven and bake it at 120°C for 12 hours, and then cut it into positive electrode sheets with a diameter of 16 mm.
[0108] Embodiment 17
[0109] The sodium ion battery positive electrode material obtained in Example 1 is used as the positive electrode active material, and a positive electrode sheet is prepared according to the following method: each raw material is weighed and mixed evenly according to the mass ratio of positive electrode active material: potassium chloride: conductive agent (Super-P): binder (PVDF) of 79.2:0.8:10:10 (that is, the mass of chloride is 1% of the mass of the sodium ion battery positive electrode material), and then solvent NMP (N-methylpyrrolidone) is added thereto, and after mixing evenly, a positive electrode slurry is obtained, which is coated on an aluminum foil, and then placed in a vacuum drying oven and baked at 120°C for 12 hours, and then cut into a positive electrode sheet with a diameter of 16 mm.
[0110] Embodiment 18
[0111] The preparation method of the positive electrode sheet provided in this embodiment is basically the same as that of Example 17, except that the sodium ion battery positive electrode material obtained in Example 7 is used as the positive electrode active material.
[0112] Embodiment 19
[0113] The preparation method of the positive electrode sheet provided in this embodiment is basically the same as that of Example 17, except that potassium chloride is replaced with an equal mass of calcium chloride.
[0114] Embodiment 20
[0115] The preparation method of the positive electrode sheet provided in this embodiment is basically the same as that of Example 17, except that the raw materials are weighed and mixed evenly according to the mass ratio of positive electrode active material: potassium chloride: conductive agent: binder of 79.6:0.4:10:10 (that is, the mass of chloride is 0.5% of the mass of the sodium ion battery positive electrode material).
[0116] Comparative Example 1
[0117] The preparation method of the sodium ion battery positive electrode material provided in this comparative example is basically the same as that in Example 1, except that 0.83 Ni 0.33 Ti 0.33 Mn 0.33 O2 weighs the raw materials in corresponding proportions, that is, the sodium ion battery positive electrode material prepared in this comparative example does not contain B.
[0118] According to the preparation method of the positive electrode sheet of Example 9, the positive electrode sheet was made using the sodium ion battery positive electrode material prepared in this comparative example.
[0119] Comparative Example 2
[0120] The preparation method of the sodium ion battery positive electrode material provided in this comparative example is basically the same as that in Example 1, except that nickel oxide is replaced by an equal molar amount of titanium dioxide, that is, the sodium ion battery positive electrode material prepared in this comparative example does not contain Ni, and its chemical formula is Na0.83 Ti 0.3 Mn 0.6 B 0.1 O2.
[0121] According to the preparation method of the positive electrode sheet of Example 9, the positive electrode sheet was made using the sodium ion battery positive electrode material prepared in this comparative example.
[0122] Comparative Example 3
[0123] The preparation method of the positive electrode material for a sodium ion battery provided in this comparative example is basically the same as that in Example 1, except that titanium dioxide is replaced by manganese tetraoxide in an equal molar amount based on the manganese element, that is, the positive electrode material for a sodium ion battery prepared in this comparative example does not contain Ti, and its chemical formula is Na 0.83 Ni 0.6 Mn 0.3 B 0.1 O2.
[0124] According to the preparation method of the positive electrode sheet of Example 9, the positive electrode sheet was made using the sodium ion battery positive electrode material prepared in this comparative example.
[0125] Comparative Example 4
[0126] The preparation method of the positive electrode material for a sodium ion battery provided in this comparative example is basically the same as that in Example 1, except that manganese tetraoxide is replaced by titanium dioxide in an equal molar amount based on the titanium element, that is, the positive electrode material for a sodium ion battery prepared in this comparative example does not contain Mn, and its chemical formula is Na 0.83 Ni 0.6 Ti 0.3 B 0.1 O2.
[0127] According to the preparation method of the positive electrode sheet of Example 9, the positive electrode sheet was made using the sodium ion battery positive electrode material prepared in this comparative example.
[0128] Experimental example
[0129] The positive electrode sheets prepared in each embodiment and each comparative example were respectively used, and 1M NaPF6 in PC=100with+3% FEC was used as the electrolyte, glass fiber was used as the separator, and the sodium sheet was used as the negative electrode sheet. CR2025 sodium ion button batteries were assembled in a glove box filled with argon. Then, the charge and discharge capacity and the first coulomb efficiency at 2-4.35V and 0.1C, as well as the reversible specific capacity at 2-4.25V and 1C and the capacity retention rate after 200 cycles were tested. The test results are shown in Table 1 below.
[0130] Table 1 Electrochemical performance
[0131]
[0132] In addition, the comparison diagram of the first charge and discharge curves of the batteries assembled with the sodium ion battery positive electrode materials prepared in Example 1, Example 2 and Example 3 at 2-4.35V, 0.1C and 2-4.25V, 1C respectively is shown in Figure 3 The 200-cycle curve comparison of the batteries assembled with the sodium ion battery positive electrode materials prepared in Example 1, Example 2 and Example 3 is shown in FIG. Figure 4 The comparison of the first charge and discharge curves of the batteries assembled with the sodium ion battery positive electrode materials of Comparative Examples 1 to 4 at 2-4.35V and 0.1C is shown in the figure below. Figure 5 The 200-week cycle curve comparison of the batteries assembled with the sodium ion battery positive electrode materials of Comparative Examples 1 to 4 is shown in FIG. Figure 6 shown.
[0133] It can be seen from Table 1 that, compared with the comparative examples, the battery capacity of each embodiment is higher and the cycle performance is better.
[0134] Specifically, by comparing Example 9 and Example 17, and Example 15 and Example 18, it can be seen that adding chloride to the positive electrode sheet can increase the capacity and the first efficiency, and can improve the cycle performance.
[0135] By comparing Example 9 with Comparative Examples 1 to 4, it can be seen that Ni, Ti, Mn, and B have a synergistic effect, and failure to add any element will result in decreased capacity or cycle performance.
[0136] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.
Claims
1. A sodium ion battery positive electrode material, characterized in that: The general formula of the sodium ion battery positive electrode material is Na w Ni x Ti y Mn z B 1-x-y-z O2; among them, 0.6≤w≤0.9, 0.2≤x≤0.5, 0.1≤y≤0.2, 0.4≤z≤0.6, 0.05≤1-xyz≤0.
25.
2. The sodium ion battery positive electrode material according to claim 1, characterized in that: At a temperature of 20 to 25° C., the pH of the aqueous solution containing 32.5% to 33.5% of the sodium ion battery positive electrode material by mass is 12.2 to 12.
75.
3. The sodium ion battery positive electrode material according to claim 1, characterized in that: The median particle size of the sodium ion battery positive electrode material is 3 to 15 μm.
4. The method for preparing a positive electrode material for a sodium ion battery according to any one of claims 1 to 3, characterized in that: The steps include: The sodium source, the nickel source, the titanium source, the manganese source and the boron source are mixed and then sintered.
5. The method for preparing the positive electrode material for a sodium ion battery according to claim 4, characterized in that: The boron source includes at least one of calcium boride, silicon boride, chromium boride, boron nitride and boron bromide.
6. The method for preparing the positive electrode material for sodium ion battery according to claim 4, characterized in that: The sintering temperature is 900-1200° C., and the heat preservation time is 15-20 hours.
7. A positive electrode sheet, characterized in that: The invention comprises the sodium ion battery positive electrode material as claimed in any one of claims 1 to 3.
8. The positive electrode sheet according to claim 7, characterized in that: The positive electrode sheet also includes chloride; Wherein, the mass of the chloride is 0.5% to 1% of the mass of the sodium ion battery positive electrode material, and / or the chloride includes at least one of potassium chloride, calcium chloride, barium chloride, ferric chloride, ferrous chloride, cupric chloride, and aluminum chloride.
9. A sodium ion battery, characterized in that: Comprising the positive electrode sheet as claimed in claim 7.
10. An electrical device, characterized in that: Comprising the sodium ion battery as claimed in claim 9.