Composite catalyst, composite lithium supplementing material and preparation method and application of composite catalyst and composite lithium supplementing material
By using a composite catalyst composed of evenly distributed biomass carbon materials and transition metal compounds in lithium-ion batteries combined with lithium-rich materials, the problem of loss of active lithium in lithium-ion batteries during the first charging and discharging process is solved, and efficient lithium supplementation is achieved and increase in energy density.
Patent Information
- Application Number
- CN202411021489.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-19
AI Technical Summary
During the first charging and discharging process of lithium-ion batteries, the formation of solid electrolyte interface films leads to irreversible loss of active lithium, resulting in a decrease in energy density, limiting the widespread application of lithium-ion batteries.
The composite catalyst is composed of biomass carbon materials and transition metal compounds, and is uniformly distributed in the biomass carbon materials. It combines lithium-rich materials to form a composite lithium supplement material. It is prepared by hydrothermal treatment and calcination treatment to improve the structural stability and conductivity of the catalyst. Performance, reduce the deliquency voltage of lithium-rich materials.
It effectively reduces the deliquification voltage of lithium-rich materials, improves the lithium supplement capacity, the first effect and energy density of the battery, and enhances the cycling performance and structural stability of the battery.
Smart Images

Figure CN118983442A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of lithium-ion batteries, and in particular relates to a composite catalyst, a composite lithium supplement material, and a preparation method and application thereof. Background Art
[0002] The intermittent and periodic nature of renewable energy seriously hinders their widespread application. An effective way to solve this problem is to convert it into chemical energy and store it. Among various energy storage systems, electrochemical energy storage is favored by people because of its high energy conversion efficiency and less space constraints. Among various electrochemical energy storage devices, secondary batteries, especially lithium-ion batteries (LIBs), have attracted widespread attention due to their high energy density and power density.
[0003] Since a solid electrolyte interface film will form on the negative electrode surface during the first charge and discharge process of LIBs, causing irreversible loss of active lithium, which in turn leads to a decrease in the capacity of the electrode material and a decrease in energy density, this seriously limits the widespread application of LIBs. By adding lithium-supplementing materials to the positive electrode material, the loss of active lithium during the first charge of LIBs can be compensated, effectively improving the energy density of LIBs. However, the delithiation potential of most lithium-supplementing materials is high and cannot match that of most commercial positive electrode materials, which seriously limits their widespread application. Summary of the invention
[0004] The purpose of the present application is to provide a composite catalyst, a composite lithium supplement material, and a preparation method and application thereof, in order to solve the problem of low catalytic activity or poor conductivity of the catalyst.
[0005] In order to achieve the above application purpose, the technical solution adopted in this application is as follows:
[0006] In a first aspect, the present application provides a composite catalyst, comprising a biomass carbon material and a transition metal compound, wherein the transition metal compound is uniformly distributed in the biomass carbon material.
[0007] In a second aspect, the present application provides a composite lithium supplement material, comprising: a lithium-rich material and the composite catalyst provided in the first aspect, wherein the composite catalyst is combined with the lithium-rich material.
[0008] In a third aspect, the present application provides a method for preparing a catalyst, comprising the following steps:
[0009] The biomass carbon source, the first metal source, and the organic matter are mixed in a solution system, and subjected to hydrothermal treatment, so that the metal ions in the first metal source coordinate with the organic matter to form a metal organic framework and combine with the carbon source to obtain a catalyst precursor;
[0010] reacting a catalyst precursor, a second metal source, and a first reaction source in a solution system to obtain a catalyst intermediate;
[0011] The catalyst intermediate and the second reaction source are mixed and calcined to obtain a composite catalyst;
[0012] The composite catalyst is mixed with the lithium-rich material to obtain a composite lithium-supplementing material.
[0013] In a fourth aspect, the present application provides a positive electrode, comprising a positive electrode active material and a lithium supplement material, wherein the lithium supplement material comprises the composite lithium supplement material provided in the second aspect and / or the composite lithium supplement material prepared by the preparation method of the composite lithium supplement material provided in the third aspect.
[0014] In a fifth aspect, the present application provides a secondary battery, comprising a positive electrode plate, a negative electrode plate and an electrolyte, wherein the positive electrode plate comprises the positive electrode in the fourth aspect.
[0015] The composite catalyst provided in the first aspect of the present application includes a biomass carbon material and a transition metal compound. Specifically, the transition metal compound is distributed in the biomass carbon material in a uniformly distributed form. On the one hand, more effective active sites can be provided, so that more transition metal compounds can participate in the catalytic reaction, so as to exert better catalytic performance, thereby effectively reducing the lithium decomposition voltage of the lithium-rich material, and on the other hand, the uniformly distributed form can avoid local stress concentration, thereby reducing the damage to the structure of the composite catalyst caused by local stress concentration, thereby increasing the structural stability of the composite catalyst; moreover, uniform distribution means that the transition metal compound is not prone to agglomeration tendency, which is more conducive to the catalytic activity of the transition metal compound. In addition, the biomass carbon material has excellent electrical conductivity, and the electronic conductive environment formed thereby is more conducive to enhancing the catalyst effect of the transition metal compound, which can better promote the lithium-rich material to fully delithiate at a lower potential, thereby improving the specific capacity of the lithium-rich material. Therefore, the composite catalyst provided by the present application has a stable structure, not only has excellent catalytic performance, but also has good electrical conductivity.
[0016] The present application combines the catalyst provided in the first aspect with a lithium-rich material to obtain a composite lithium-supplementing material. On the one hand, based on the structure of the composite catalyst, since the content of transition metal compounds in the composite catalyst is higher, in lithium-supplementing materials of the same volume, the catalytic effect of the composite catalyst on the lithium-rich material in the composite lithium-supplementing material provided by the present invention is enhanced, so that the decomposition voltage of the lithium-rich material decreases more significantly; on the other hand, the lithium-rich material is combined with the composite catalyst, which gives the composite lithium-supplementing material excellent structural stability, which is more conducive to the performance and enhancement of the catalytic effect of the composite catalyst, so that the decomposition voltage of the lithium-rich material can be further reduced.
[0017] The preparation method of the composite lithium supplement material provided in the third aspect of the present application is to construct a metal organic framework combined with a carbon source by combining an organic ligand and a metal ion, and then perform a chemical reaction and calcination treatment to make the transition metal compound evenly distributed on the biomass carbon material to obtain a composite catalyst; finally, the composite catalyst is mixed with a lithium-rich material to effectively prepare a composite lithium supplement material having the properties of the composite lithium supplement material of the present application as described above. In addition, the preparation method of the composite lithium supplement material of the present application can ensure that the structure and electrochemical properties of the prepared composite lithium supplement material are stable, so that the lithium supplement performance can be fully exerted, and the composite lithium supplement material is endowed with excellent lithium removal ability, so as to achieve efficient lithium supplementation of the battery, which is conducive to wide application.
[0018] The positive electrode provided in the fourth aspect of the present application contains the composite lithium replenishing material of the present application, and the composite lithium replenishing material can delithium at a low delithiation voltage, has good stability, and has a high lithium replenishing capacity. It can replenish the lithium ions consumed by the SEI film during the first charge and discharge. Therefore, the positive electrode of the present application has a high lithium replenishing capacity, thereby improving the initial efficiency and energy density of the battery containing the positive electrode material of the present application.
[0019] The secondary battery provided in the fifth aspect of the present application contains the positive electrode of the present application, so the secondary battery of the present application has high first efficiency and energy density, and its cycle performance is stable. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0021] Figure 1 is a schematic diagram of the structure of the composite catalyst provided in the examples of the present application;
[0022] Figure 2 It is a schematic diagram of the structure of the composite lithium supplement material provided in the embodiment of the present application.
[0023] Among them, the reference numerals in the figure are:
[0024] 100. Composite catalyst, 200. Composite lithium supplement material;
[0025] 10. Biomass carbon materials, 20. Porosity, 30. Transition metal compounds, 40. Lithium-rich materials. DETAILED DESCRIPTION
[0026] In order to make the technical problems, technical solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0027] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.
[0028] In this application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.
[0029] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.
[0030] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "said" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.
[0031] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass described in the embodiment description of the present application can be a mass unit known in the chemical industry such as μg, mg, g, kg, etc.
[0032] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of indicated technical features. For example, without departing from the scope of the embodiments of the present application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features.
[0033] The term "MOF" is the abbreviation of "Metal organic Framework", which means metal organic framework. It is the abbreviation of metal organic framework compounds. It is a crystalline porous material with a periodic network structure formed by inorganic metal centers (metal ions or metal clusters) and bridging organic ligands that are interconnected through self-assembly.
[0034] A first aspect of an embodiment of the present application provides a composite catalyst, comprising a biomass carbon material and a transition metal compound, wherein the transition metal compound is uniformly distributed in the biomass carbon material.
[0035] See also Figure 1 The composite catalyst 100 includes a biomass carbon material 10 and a transition metal compound 30 , and the transition metal compound 30 is uniformly distributed in the biomass carbon material 10 .
[0036] Specifically, the composite catalyst acts on the lithium-rich material to catalytically reduce the lithium-desorption potential of the lithium-rich material and improve the conductivity of the lithium-rich material. It is understandable that the composite catalyst can be mixed with the lithium-rich material and contacted with the lithium-rich material to achieve a catalytic effect. The biomass carbon material in the composite catalyst can be used to improve the electronic conductivity and ionic conductivity of the lithium-rich material, and the transition metal compound in the composite catalyst can be used to reduce the lithium-desorption potential of the lithium-rich material, so that the lithium-rich material can release lithium ions at a lower potential.
[0037] It is understood that biomass carbon materials refer to carbon materials with certain structures and properties that are converted from biomass carbon sources under anaerobic or hypoxic conditions through pyrolysis, carbonization and other treatment methods. Biomass carbon materials contain more pores and a large number of functional groups (such as carboxyl groups), which are conducive to the adsorption of metal ions.
[0038] It is understood that uniform distribution means that in a specific space or region, the transition metal compound presents a dispersed and relatively balanced state. In the embodiment of the present application, uniform distribution means that the transition metal compound is distributed in the biomass carbon material, presenting a non-agglomerated and non-concentrated distribution state, which means that there is no obvious difference in the distribution of the transition metal compound between the various parts of the biomass carbon material, and there is no obvious aggregation or agglomeration phenomenon.
[0039] The composite catalyst provided in the first aspect of the embodiment of the present application includes a biomass carbon material and a transition metal compound. Based on the specific structure of the biomass carbon material, it is more conducive to the adsorption of the transition metal compound. In this way, the binding force between the transition metal compound and the biomass carbon material is strong, so that the transition metal compound is not easy to fall off, reducing the loss of the transition metal compound; in particular, the transition metal compound is distributed in the biomass carbon material in a uniformly distributed form. On the one hand, it can provide more effective active sites, so that more transition metal compounds can participate in the catalytic reaction, so as to play a better catalytic performance, thereby effectively promoting the decomposition of the lithium-rich material, so that the decomposition voltage of the lithium-rich material drops more significantly, on the other hand, the uniformly distributed form can avoid local stress concentration, thereby reducing the damage to the composite catalyst structure caused by local stress concentration, thereby increasing the structural stability of the composite catalyst; and, uniform distribution means that the transition metal compound is not easy to produce agglomeration tendency, which is more conducive to the catalytic activity of the transition metal compound. In addition, the biomass carbon material has excellent electrical conductivity, and the electronic conductive environment formed thereby is more conducive to enhancing the catalyst effect of the transition metal compound, which can better promote the lithium-rich material to fully remove lithium at a lower potential, thereby improving the specific capacity of the lithium-rich material. Therefore, biomass carbon materials can play a synergistic role with transition metal compounds to improve the comprehensive performance of the composite catalyst, so that the composite catalyst can better promote the full delithiation of lithium-rich materials at a lower potential, thereby increasing the specific capacity of lithium-rich materials.
[0040] In some embodiments, the biomass carbon material has a porous structure, and the transition metal compound is distributed in the porous structure of the biomass carbon material.
[0041] The biomass carbon material has a porous structure, which makes the biomass carbon material have more active sites, which is conducive to the attachment of transition metal compounds. That is, the biomass carbon material can use its own structure to firmly combine the biomass carbon material with the transition metal compound. The transition metal compound is not easy to fall off from the biomass carbon material, so that the composite catalyst has a higher structural stability.
[0042] The pore structure of the biomass carbon material can provide sufficient accommodation space for accommodating the transition metal compound, so that the transition metal compound is not easy to fall off, thereby effectively improving the structural stability of the composite catalyst.
[0043] In some embodiments, the transition metal compound is distributed on the surface of the biomass carbon material.
[0044] The transition metal compound can be independently distributed on the outer surface of the biomass carbon material to form a discontinuous point distribution, and the particles of the transition metal compound are independent of each other.
[0045] See also Figure 1The biomass carbon material 10 has a plurality of pores 20 , and the transition metal compound 30 may be attached to the outer surface of the biomass carbon material 10 , or the transition metal compound 30 may be distributed in the pores 20 .
[0046] In some embodiments, the biomass carbon material is doped with at least one non-metallic element selected from the group consisting of S, N, and P.
[0047] By doping with non-metallic elements, the electronic structure and surface polarity of biomass carbon materials can be changed, thereby improving the conductivity and catalytic activity of the composite catalyst; the doped biomass carbon materials can play a synergistic role with transition metal compounds to improve the comprehensive performance of the composite catalyst. In addition, the doped non-metallic elements can also serve as delithiation sites, thereby promoting the insertion and extraction of lithium ions in lithium-rich materials.
[0048] In some embodiments, the mass proportion of the doping element in the biomass carbon material is 0.06%-0.6%, and a further optional range is 0.2%-0.3%. Exemplarily, the doping element includes at least one of S, N, and P.
[0049] Controlling the doping amount of the doping element within the above range enhances the electron transport capability of the biomass carbon material; and using it in combination with a transition metal compound can produce a better catalytic effect.
[0050] In some embodiments, the transition metal compound contains at least two different transition metal compounds, and a heterojunction is formed between the two transition metal compounds.
[0051] A heterojunction is formed between two or more transition metal compounds, and a special electron transfer path can be formed at the heterojunction interface to promote electron transfer, which can further promote the decomposition of lithium-rich materials and make the decomposition voltage of lithium-rich materials drop more significantly.
[0052] A variety of transition metal compounds can form a good synergistic effect, effectively reducing the barrier for the decomposition of lithium-rich materials, allowing them to decompose at a lower potential and release capacity. In addition, heterojunctions can make the contact between transition metal compounds better, which is more conducive to catalytic effects.
[0053] The position of the heterojunction should depend on the position of the transition metal compound. For example, when the transition metal compound is evenly distributed on the outer surface of the biomass carbon material, the heterojunction should also be evenly distributed on the outer surface of the biomass carbon material. Of course, when the transition metal compound is distributed inside the biomass carbon material, the heterojunction can be formed inside the biomass carbon material.
[0054] In some embodiments, the transition metal compound includes one or more of a transition metal compound, a transition metal selenide, a transition metal phosphide, and the like.
[0055] These transition metal compounds have good catalytic ability for lithium-rich materials and can effectively reduce the decomposition voltage of lithium-rich materials.
[0056] In some embodiments, the corresponding transition metal in the transition metal compound includes at least two of Fe, Mo, and Co.
[0057] Exemplarily, the transition metal compound includes at least two of molybdenum disulfide, cobalt tetrasulfide, and iron cobalt sulfide. For example, molybdenum disulfide and cobalt tetrasulfide can form a PP heterostructure, thereby effectively reducing the decomposition barrier of the lithium-rich material, which is conducive to the decomposition of the lithium-rich material at a lower potential and releasing capacity.
[0058] The electronic interaction between different metal atoms in iron-cobalt sulfide can adjust the electronic structure of the third transition metal compound, making it have better conductivity; and its bimetallic structural characteristics make it show higher activity in catalytic reactions.
[0059] In some embodiments, the loading amount of the transition metal compound on the biomass carbon material is 80%-400%, and the further optional range is 100%-200%. Exemplarily, the loading amount of the transition metal compound on the biomass carbon material can be 80%, 100%, 150%, 200%, 300%, 350%, 400% and other typical but non-limiting values.
[0060] The loading capacity refers to the amount of other substances that a material carries, contains or supports in a specific system or environment. In the embodiments of the present application, the loading capacity refers to the amount of transition metal compounds that the biomass carbon material can accommodate. For example, a loading capacity of 100% means that 1g of biomass carbon material can accommodate 1g of transition metal compounds.
[0061] Satisfying the loading amount of the transition metal compound on the biomass carbon material to be within the above range means that the content of the transition metal compound on the biomass carbon material is higher, and it is easier to play an effective catalytic role.
[0062] In some embodiments, the density of the composite catalyst is 6.4 g / cm 3 -10g / cm 3 , the density standard deviation of the composite catalyst is 0.6-0.9. Exemplarily, the density of the composite catalyst can be 6.4 g / cm 3 , 7g / cm 3 , 7.5g / cm 3 , 8g / cm 3 、8.5g / cm3 , 9g / cm 3 , 9.5g / cm 3 、10g / cm 3 etc. are typical but not limiting values.
[0063] Since there is a significant difference in density between transition metal compounds and biomass carbon materials, there is a certain fluctuation in the value when measuring the density of the composite catalyst. The density of the composite catalyst mentioned above refers to the average value of the density obtained from multiple measurements.
[0064] Density standard deviation is a statistic that reflects the degree of dispersion of a set of material density data. It can measure the fluctuation of material density around its average value. When the standard deviation is large, it means that the density difference of these samples is large, which may mean that the composition and structure of the composite catalyst material are relatively non-uniform. On the contrary, a smaller standard deviation means that these densities are relatively close to the average value, and the density consistency of the composite catalyst is better, which means that the distribution of transition metal compounds in the composite catalyst is uniform.
[0065] In some embodiments, the D50 particle size of the transition metal compound is 50 nm-1000 nm. Exemplarily, the D50 particle size of the transition metal compound can be 50 nm, 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm, 1000 nm, etc., which are typical but non-limiting values.
[0066] Controlling the D50 particle size of the transition metal compound within the above range is conducive to the combination of the transition metal compound and the biomass carbon material, making it difficult for the transition metal compound to fall off, reducing the loss of the transition metal compound, and thereby improving the catalytic effect of the composite catalyst.
[0067] In some embodiments, the specific surface area of the biomass carbon material is 10 m 2 / g-500m 2 / g. Exemplarily, the specific surface area of the biomass carbon material can be 10m 2 / g, 50m 2 / g、100m 2 / g, 200m 2 / g、300m 2 / g, 400m 2 / g、500m 2 / g and other typical but non-limiting values.
[0068] Specific surface area refers to the total area per unit mass of a substance.
[0069] The specific surface area of the biomass carbon material is within the above range, which means that the biomass carbon material has a relatively large porous structure, so that it can adsorb as many transition metal compounds as possible, which is beneficial to the loading of the transition metal compounds.
[0070] In some embodiments, the diameter of the biomass carbon material is 0.6 μm-10 μm, and the length is 10 μm-40 μm. Exemplarily, the diameter of the biomass carbon material can be 0.6 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 4 μm, 4.5 μm, 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 7.5 μm, 8 μm, 8.5 μm, 9 μm, 9.5 μm, 10 μm, etc. Typical but non-limiting values. The length of the biomass carbon material can be 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, etc. Typical but non-limiting values.
[0071] The biomass carbon material includes one or more of rod-shaped, fibrous, cylindrical and spindle-shaped shapes. Specifically, the biomass carbon material can be in a three-dimensional shape such as rod-shaped, fibrous, cylindrical, etc. This shape is conducive to loading transition metal compounds and makes the loading amount of transition metal compounds at a higher level, thereby making it easier to improve the catalytic activity of the composite catalyst.
[0072] A third aspect of the present application provides a composite lithium supplement material, including:
[0073] Lithium-rich materials, and
[0074] The composite catalyst provided in the first aspect of the present application is combined with a lithium-rich material.
[0075] See also Figure 2 The composite lithium supplement material 200 includes a lithium-rich material 40 and a composite catalyst 100 . The composite catalyst 100 includes a biomass carbon material 10 and a transition metal compound 30 uniformly distributed on the biomass carbon material 10 .
[0076] Specifically, lithium-rich materials can be used to supplement lithium, and the lithium-rich materials can be in a granular form, including a spherical or quasi-spherical shape. The lithium-rich material can be a primary particle, or a secondary particle formed by the aggregation of primary particles. During the first charging process, the lithium (Li) in the lithium-rich material can be released and migrated to the negative electrode of the battery to offset the irreversible lithium loss caused by the formation of the SEI film, thereby ensuring the abundance of lithium ions in the battery system and improving the total capacity and energy density of the battery.
[0077] In some embodiments of the present application, the lithium-rich material 40 includes an organic lithium salt, whose chemical formula is Li x1 C y1 O z1, where 0 < x1 ≤ 2, y1 > 0, z1 > 0. In some embodiments of the present application, the lithium-rich material 40 may include one or more of Li2C3O3, Li2C4O4, Li2C6O6, Li2C3O5, Li2C2O4, and Li2C4O6. It can be understood that the lithium-rich materials of lithium oxalate have a high theoretical capacity (> 525 mAh g -1 ), and good air stability, and are considered to be an extremely attractive cathode prelithiation additive.
[0078] In some embodiments of the present application, the lithium-rich material 40 further includes other lithium-supplementing materials with a higher decomposition voltage, mainly including lithium-supplementing materials with a delithiation potential above 4V, such as Li2O (delithiation potential 4.5V), Li2O2 (delithiation potential 4.3V), LiOH (delithiation potential 4.8V), Li4SiO4 (delithiation potential 4.5V), Li3PO4 (delithiation potential exceeding 4V), Li2CO3 (delithiation potential 4.7V), Li5FeO4 (delithiation potential 4V).
[0079] The above-mentioned lithium-rich materials all have a high capacity, but the delithiation of these lithium-rich materials requires a high charging voltage, and there is a technical problem of a high platform voltage. At the same time, the high voltage also causes oxygen to be generated during the first charge and discharge of the lithium-rich material in the lithium-ion battery, and the generated oxygen further oxidizes and decomposes the electrolyte, resulting in a reduction in the safety and performance of the lithium-ion battery. These lithium-rich materials with a higher decomposition voltage are also difficult to be compounded with conventional cathode materials (such as the delithiation potential of lithium iron phosphate is about 3.5V), which limits the wide application of the lithium-supplementing materials. Therefore, in the present application, by utilizing the catalytic effect of the transition metal compound, and further through the heterostructure of the transition metal compound, a special electron transfer path is formed at the heterojunction interface, thereby promoting electron transfer, effectively promoting the decomposition of the lithium-rich material, and reducing the decomposition voltage; in addition, the catalytic effect of the transition metal compound is strengthened by the conductivity of the biomass carbon material, so that the decomposition voltage of the lithium-rich material is significantly reduced.
[0080] Optionally, the lithium-rich material 40 may further include a binary lithium-supplementing agent and / or a ternary lithium-supplementing agent. The chemical general formula of the lithium-rich material 40 corresponding to the binary lithium-supplementing agent is Li x2 M y2 , where M is at least one element of S, P, N, F, B, Se, Te, 1 ≤ x2 ≤ 5, 0 < y2. The binary lithium-supplementing agent includes but is not limited to at least one of Li3N, Li2S, LiF, Li3P, and Li2Se.
[0081] Optionally, the chemical formula of the ternary lithium-supplementing agent is represented as Li a M b O c, where M is at least one element among Fe, Ni, Mn, Cu, Zn, Co, Cr, Zr, Sb, Ti, V, Mo, Sn, etc., 1 ≤ a ≤ 8, 0 < b, 0 < c < 7. In a specific embodiment, the lithium-rich material 40 can be Li5FeO4, Li6MnO4, Li6CoO4, Li6ZnO4, Li2NiO2, Li2CuO2, Li2CoO2, Li2MnO2, Li2Ni 0.5 Mn 1.5 O4, Li2Ni d Cu (1-d) O2 (0 < d < 1), etc.
[0082] The chemical formula of the lithium-rich material 40 can also be expressed as Li 1+x3 A y3 O z3 , where 0 < x3 ≤ 1.2, 1 ≤ y3 < 3, z3 > 0, and A includes at least one of Ni, Fe, Mn, Co, Cr, V, Mo, Ti, Nb, Zr, Cu, Mg. These lithium-rich materials 40 can be used as a lithium supplement agent or directly as a cathode material. Exemplarily, the lithium-rich material 40 includes at least one of Li2CuO2, Li2NiO2, Li2MnO2.
[0083] The above-mentioned lithium-rich materials can be undoped or doped and modified, or can be surface-coated, prelithiated, etc. In the embodiments of the present invention, when the lithium-rich material is used as a cathode active material, the lithium-rich material can also be a combination of the above-listed lithium-rich materials and conventional cathode materials such as lithium iron phosphate and ternary cathode materials.
[0084] Optionally, the combination of the lithium-rich material and the composite catalyst can be: the lithium-rich material is combined with the biomass carbon material in the composite catalyst. For example, the lithium-rich material adheres to the outer surface of the biomass carbon material, or can also be distributed inside the biomass carbon material; or, the lithium-rich material is combined with the transition metal compound in the composite catalyst. For example, the lithium-rich material is in contact with the transition metal compound.
[0085] In the embodiments of the present application, by combining the catalyst provided in the first aspect with the lithium-rich material to obtain a composite lithium supplement material. On the one hand, based on the structure of the catalyst, since the content of the transition metal compound in the composite catalyst is higher, in the lithium supplement material of the same volume, the catalytic effect of the composite catalyst on the lithium-rich material in the composite lithium supplement material provided by the present invention is enhanced, making the decomposition voltage of the lithium-rich material decrease more significantly; on the other hand, the combination of the lithium-rich material and the composite catalyst endows the composite lithium supplement material with excellent structural stability, which is more conducive to the exertion and enhancement of the catalytic effect of the composite catalyst, so that the decomposition voltage of the lithium-rich material can be further reduced.
[0086] In some embodiments, the lithium-rich material is uniformly distributed in the composite catalyst.
[0087] Since the composite catalyst has more active sites, the lithium-rich material preferentially combines with the transition metal compound during the combination with the composite catalyst; since the transition metal compound is evenly distributed in the composite catalyst, the lithium-rich material is also evenly distributed in the biomass carbon material.
[0088] In some embodiments, the biomass carbon material includes one or more of a rod, a fiber, a cylinder and a spindle. Specifically, the biomass carbon material can be in a three-dimensional shape such as a rod, a fiber, a cylinder, etc. This shape is not only conducive to the biomass carbon material loading the transition metal compound to form a composite catalyst, thereby making the loading amount of the transition metal compound at a higher level, thereby making it easier to improve the catalytic activity of the composite catalyst, but also conducive to the composite catalyst formed to combine with the lithium-rich material, under the catalytic action of the composite catalyst, the decomposition voltage of the lithium-rich material drops more significantly.
[0089] In some embodiments, a portion of the lithium-rich material is attached to the transition metal compound.
[0090] Part of the lithium-rich material is attached to the transition metal compound, which means that part of the lithium-rich material is in contact with the transition metal compound, so that the transition metal compound and the lithium-rich material have a larger contact area, which is conducive to the transition metal compound to play a catalytic role, effectively reducing the decomposition voltage of the lithium-rich material, so that the lithium-rich material can decompose and produce lithium ions at a lower potential. In one embodiment, the lithium-rich material and the transition metal compound are in a granular form, and the lithium-rich material is in contact with one or more transition metal compounds, so that the effect of releasing lithium from the lithium-rich material can be improved.
[0091] In some embodiments, the biomass carbon material has a porous structure, and part of the lithium-rich material is distributed in the pores of the biomass carbon material.
[0092] The pore structure of the biomass carbon material can provide enough space to accommodate the lithium-rich material, so that the lithium-rich material is fixed in the biomass carbon material and is not easy to lose, thereby increasing the capacity of the composite lithium-supplementing material; in addition, the voids of the biomass carbon material can form a confined structure, which is conducive to obtaining lithium-rich materials with smaller particle sizes, thereby improving the lithium-supplementing performance of the composite lithium-supplementing material and reducing the overpotential. In one embodiment, the transition metal compound contacts the lithium-rich material and is confined in the same pore of the biomass carbon material. At this time, the transition metal compound and the lithium-rich material have a large contact area, which can effectively reduce the decomposition potential of the lithium-rich material to better promote the delithiation of the composite lithium-supplementing material.
[0093] The porous structure of biomass carbon materials is also conducive to the infiltration of battery electrolytes and the rapid migration of electrolyte ions, which is conducive to the use of composite lithium supplement materials. In addition, the pore structure of biomass carbon materials can also absorb the gas generated by lithium-rich materials during the charging and discharging process, thereby effectively inhibiting the volume expansion of lithium-rich materials caused by gas production, and greatly improving the safety performance of batteries. Among them, the pores contained in the porous structure can be evenly distributed in the biomass carbon material, or randomly distributed.
[0094] In some embodiments, a portion of the lithium-rich material is distributed on the outer surface of the biomass carbon material.
[0095] The lithium-rich material can be independently distributed on the outer surface of the biomass carbon material to form a discontinuous point distribution, and the particles of the lithium-rich material are independent of each other.
[0096] The lithium-rich material is attached to the outer surface of the biomass carbon material, which can not only greatly reduce the risk of lithium-rich material agglomeration, but also shorten the transmission path of lithium ions, thereby facilitating the increase of the deintercalation rate of the lithium-rich material and achieving efficient lithium replenishment. In one embodiment, the transition metal compound is in contact with the lithium-rich material and attached to the outer surface of the biomass carbon material. At this time, the biomass carbon material provides an excellent conductive environment, and the transition metal compound and the lithium-rich material have a large contact area, which is more conducive to the catalytic effect of the composite catalyst, so that the lithium-rich material can be delithiated at a lower potential, thereby achieving efficient lithium replenishment.
[0097] See also Figure 2 The biomass carbon material 10 has a plurality of pores 20 , and the lithium-rich material 40 may be attached to the outer surface of the biomass carbon material 10 , or the lithium-rich material 40 may be distributed in the pores 20 .
[0098] In some embodiments, the mass ratio of the lithium-rich material to the transition metal compound in the composite catalyst and the biomass carbon material is 40-90:5-50:5-20.
[0099] The transition metal compound in the composite catalyst is used to catalytically reduce the lithium decomposition potential of the lithium-rich material, so that the lithium-rich material can release lithium ions at a lower potential. In addition, the transition metal compound does not contribute lithium ions. Therefore, the mass proportion of the transition metal compound in the embodiment of the present application is controlled within the above range, and the composite catalyst can give full play to the catalytic effect, reduce the decomposition voltage of the lithium-rich material, thereby effectively improving the capacity utilization of the lithium-rich material. Exemplarily, the mass proportion of the transition metal compound can be 5, 10, 20, 30, 40, 50, etc., which are typical but non-limiting values.
[0100] Biomass carbon material as a carrier can load lithium-rich material and transition metal compound, firmly combine lithium-rich material, biomass carbon material and transition metal compound, and provide an excellent conductive environment. In addition, biomass carbon material does not contribute lithium ions. Therefore, the embodiment of the present application controls the mass proportion of biomass carbon material within the above range, so that the composite lithium supplement material has excellent conductivity, high gram capacity and high structural stability. Exemplarily, the mass proportion of biomass carbon material can be 5, 8, 10, 15, 20 and other typical but non-limiting values.
[0101] In some embodiments, the D50 particle size of the lithium-rich material is 100 nm-1000 nm. Exemplarily, the D50 particle size of the lithium-rich material can be 100 nm, 200 nm, 300 nm, 400 nm, 500 nm, 600 nm, 700 nm, 800 nm, 900 nm, 1000 nm, etc., which are typical but non-limiting values.
[0102] The D50 particle size is the particle size corresponding to when the cumulative particle size distribution percentage of the particles reaches 50%, and can be tested using methods known in the art. Controlling the D50 particle size of the lithium-rich material within the above range is conducive to the loading of the lithium-rich material in the biomass carbon material, and is also conducive to the full contact between the transition metal compound and the lithium-rich material. It can also increase the lithium content in the lithium-rich material and improve the lithium replenishment performance of the composite lithium replenishment material.
[0103] A third aspect of the present application provides a method for preparing a composite lithium supplement material, comprising the following steps:
[0104] Step S10, mixing a biomass carbon source, a first metal source, and an organic matter in a solution system, and performing a hydrothermal treatment, so that the metal ions in the first metal source coordinate with the organic matter to form a metal organic framework and combine with the carbon source to obtain a catalyst precursor;
[0105] Step S20, subjecting the catalyst precursor, the second metal source, and the first reaction source to a sulfurization reaction in a solution system to obtain a catalyst intermediate;
[0106] Step S30, mixing the catalyst intermediate and the second reaction source and performing calcination treatment to obtain a composite catalyst;
[0107] Step S40: Mix the composite catalyst and the lithium-rich material to obtain a composite lithium-supplementing material.
[0108] The preparation method of the composite lithium supplement material provided in the third aspect of the embodiment of the present application is to construct a metal organic framework combined with a carbon source by combining an organic ligand and a metal ion, and then perform a chemical reaction and calcination treatment to make the transition metal compound evenly distributed on the biomass carbon material to obtain a composite catalyst; finally, the composite catalyst is mixed with a lithium-rich material to effectively prepare a composite lithium supplement material having the properties of the composite lithium supplement material of the present application as described above. In addition, the preparation method of the composite lithium supplement material of the application can ensure that the structure and electrochemical properties of the prepared composite lithium supplement material are stable, so that the lithium supplement performance can be fully exerted, and the composite lithium supplement material is endowed with excellent lithium removal ability, so as to achieve efficient lithium supplementation of the battery, which is conducive to wide application.
[0109] In some embodiments, in step S10, the biomass carbon source includes a biomass material, and illustratively, the biomass carbon source includes at least one of lignin, fruit shells, and crop straw. The biomass carbon source can adsorb the metal ions contained in the first metal source, thereby facilitating the metal organic framework formed by the metal ions and the organic ligands to be anchored on the biomass carbon source.
[0110] In some embodiments, in step S10, the first metal source includes at least one of an iron source and a cobalt source.
[0111] Specifically, the iron source includes a soluble iron salt. Exemplarily, the iron source includes at least one of ferric nitrate, ferric sulfate, ferric phosphate, ferric chloride and ferric oxalate.
[0112] Specifically, the cobalt source includes a soluble cobalt salt. Exemplarily, the cobalt source includes at least one of cobalt nitrate, cobalt chloride, cobalt acetate, and cobalt sulfate.
[0113] In some embodiments, in step S10, the step of mixing the biomass carbon source, the first metal source, and the organic matter in a solution system and performing a hydrothermal treatment so that the metal ions in the first metal source coordinate with the organic matter to form a metal organic framework and combine with the carbon source comprises:
[0114] Step S11, adding the biomass carbon source, the first iron source, and the first cobalt source into deionized water, mixing, and immersing to obtain a pretreated carbon source;
[0115] Step S12, adding the organic matter, the second iron source, and the second cobalt source into a solvent to form a raw material solution;
[0116] Step S13, adding the pretreated carbon source to the raw material liquid, transferring it to a hydrothermal reactor, and performing a hydrothermal reaction. After the reaction is completed, the catalyst precursor is obtained by centrifugal washing and drying.
[0117] In step S10, the biomass carbon source is first pre-adsorbed with metal ions such as iron ions and cobalt ions, and then the biomass carbon source is mixed with a raw material liquid containing metal ions and organic matter for a hydrothermal reaction. At this time, the metal ions and the organic ligands form a MOF material, and because the metal ions are adsorbed in the biomass carbon source, the MOF material is combined with the biomass carbon source, that is, the MOF material is anchored on the biomass carbon source.
[0118] Specifically, in step S11, the immersion treatment time is 24h-48h.
[0119] Specifically, in step S11, the total concentration of metal ions in the mixed solution used for the immersion treatment is 50-70 mmol / L. The molar ratio of iron atoms contained in the first iron source to cobalt atoms contained in the first cobalt source is 0.8-1.2:0.8-1.2.
[0120] Specifically, in step S12, the molar ratio of the organic matter, the iron atoms contained in the second iron source, and the cobalt atoms contained in the second cobalt source is 0.2:1.8-2.2:0.8-1.2.
[0121] Specifically, in step S12, the solvent includes dimethylformamide, ethanol and deionized water, and the volume ratio of dimethylformamide, ethanol and deionized water is 8-12:1-3:0.5-1.5.
[0122] Specifically, in step S13, the hydrothermal reaction conditions are: temperature of 110° C.-130° C., and time of 22 h-26 h.
[0123] Specifically, in step S13, washing is performed using anhydrous ethanol.
[0124] Specifically, in step S13, the drying temperature is 60°C-65°C.
[0125] In some embodiments, in step S20, the step of subjecting the catalyst precursor, the second metal source, and the first reaction source to a sulfurization reaction in a solution system comprises:
[0126] Step S21, adding a catalyst precursor, a second metal source, and a first reaction source into ethanol respectively to obtain a reaction solution;
[0127] Step S22, transferring the reaction liquid to an autoclave for chemical reaction, and after the reaction is completed, washing and drying by centrifugation to obtain a catalyst intermediate.
[0128] In step S20, the second metal source reacts chemically with the first reaction source to obtain a second transition metal compound, and the metal ions in the catalyst precursor also react chemically to obtain a first transition metal compound. At this time, a heterostructure is formed between the first transition metal compound and the second transition metal compound.
[0129] Specifically, in step S21, the first reaction source may be at least one of a sulfur source, a selenium source, and a phosphorus source.
[0130] At this time, the metal ions contained in the second metal source and the catalyst precursor may undergo a sulfurization reaction with the sulfur source, a selenization reaction with the selenium source, or a phosphation reaction with the phosphorus source.
[0131] Exemplarily, the first reaction source includes a first sulfur source, and the first sulfur source includes but is not limited to thioacetamide. Then, the first transition metal compound includes Co3S4, and the second transition metal compound includes MoS2.
[0132] Specifically, in step S21, the second metal source includes a molybdenum source, which includes but is not limited to sodium molybdate.
[0133] Specifically, in step S21, the mass ratio of the catalyst precursor, the second metal source and the first reaction source is 1:0.4-0.6:3.4-4.5.
[0134] Specifically, in step S22, the chemical reaction varies according to the first reaction source. For example, when the first reaction source is a sulfur source, the reaction conditions include: reacting at 110°C-130°C for 3h-5h, and then reacting at 190°C-210°C for 7h-9h.
[0135] Specifically, in step S22, the drying conditions are: temperature of 60°C-65°C, and time of 7h-8h.
[0136] In some embodiments, in step S30, the biomass carbon source in the catalyst intermediate is calcined to form a biomass carbon material doped with sulfur, and the organic ligands contained in the organic metal framework bound to the surface of the biomass carbon source are gasified and cracked after calcination. The remaining metal ions in the organic metal framework are converted into metal elements and react with the second reaction source to form a third transition metal compound, and the formed third transition metal compound is bound to the biomass carbon material.
[0137] Specifically, in step S30, the second reaction source may be at least one of a sulfur source, a selenium source, and a phosphorus source.
[0138] Exemplarily, the second reaction source is a second sulfur source, which includes but is not limited to sulfur powder. In this case, the third transition metal compound Fe 0.92 Co 0.08 S.
[0139] Specifically, in step S30, the mass ratio of the catalyst intermediate to the second reaction source is 0.2-0.4:0.8-1.2.
[0140] Specifically, in step S30, the equipment used for the calcination treatment includes but is not limited to a tubular furnace. The catalyst intermediate is placed in the center of the tubular furnace, and the second reaction source is placed upstream of the tubular furnace.
[0141] Specifically, in step S30, the calcination treatment conditions include heating at a rate of 2-3°C / min. -1 The reaction was carried out at 280-320°C for 2h-3h, at 480-520°C for 2h-3h, and finally at 680-720°C for 3h-5h under an inert atmosphere.
[0142] In some embodiments, in step S40, the step of mixing the composite catalyst and the lithium-rich material to obtain the composite lithium-supplementing material includes:
[0143] The composite catalyst is placed in a saturated aqueous solution of a lithium-rich material, ultrasonically dispersed, and then ethanol is added. The precipitate is collected by filtration and dried to obtain a composite lithium-supplementing material.
[0144] The lithium-rich material is recrystallized to combine the lithium-rich material with the composite catalyst. The lithium-rich material can be attached to the transition metal compound, the outer surface of the biomass carbon material, or distributed in the pores of the biomass carbon material.
[0145] Specifically, in step S40, the selection of the lithium-rich material is as described above and will not be repeated here.
[0146] It should be noted that when the lithium-rich material is an insoluble metal compound, the lithium-rich material can also be combined with the composite catalyst by degassing or ball milling to form a composite lithium-supplementing material.
[0147] A fourth aspect of the embodiments of the present application provides a positive electrode, including a positive electrode active material and a lithium supplement material, wherein the lithium supplement material includes the composite lithium supplement material provided in any of the above embodiments.
[0148] In some embodiments, the positive electrode active material includes, but is not limited to, lithium iron phosphate, lithium iron manganese phosphate, ternary positive electrode materials (such as NCM ternary or NCA ternary), binary positive electrode materials, or lithium-rich positive electrode materials. Exemplarily, the positive electrode active material can be one or more of lithium cobalt oxide, lithium manganese oxide, lithium iron phosphate, lithium iron manganese phosphate, lithium vanadium phosphate, lithium vanadium oxyphosphate, fluorolithium vanadium phosphate, lithium nickel cobalt manganese oxide, and lithium nickel cobalt aluminum oxide.
[0149] In some embodiments, the content of the lithium supplement material in the positive electrode material can be controlled to be 1% to 6% of the mass of the positive electrode active material. For example, the mass percentage of the lithium supplement material can be 1%, 2%, 3%, 4%, 5%, 6%, etc., which are typical but non-limiting values.
[0150] This ratio can just make up for the loss of active lithium in the battery during the first charge. If the amount of lithium-supplementing material added to the positive electrode material is too low, the active lithium lost in the positive electrode active material cannot be fully replenished, which is not conducive to improving the energy density and capacity retention rate of the battery. If the amount of lithium-supplementing material added to the positive electrode active material is too high, the original reversible capacity will be occupied and the cost will increase.
[0151] A fifth aspect of an embodiment of the present application provides a secondary battery, which includes a positive electrode plate, a negative electrode plate and an electrolyte, wherein the positive electrode plate includes the positive electrode in the fourth aspect of the present application; the electrolyte can be an electrolyte solution, so the secondary battery also includes a diaphragm arranged between the positive electrode plate and the negative electrode plate; or, the electrolyte can be a solid electrolyte solution, so the secondary battery does not have a diaphragm and is replaced by a solid electrolyte.
[0152] In some embodiments, the positive electrode plate includes a positive electrode current collector and a positive electrode active layer bonded to at least one surface of the positive electrode current collector, and the positive electrode active layer includes the composite lithium replenishing material of any one of the above embodiments and / or the composite lithium replenishing material obtained by the preparation method of the composite lithium replenishing material in the above embodiments.
[0153] In some embodiments, the positive electrode sheet includes a positive current collector, and the positive current collector has a positive active layer. In addition to the positive active material and the composite lithium supplement material, the positive active layer also includes components such as a conductive agent and a binder. The present invention does not specifically limit these materials, and suitable materials can be selected according to actual application requirements. Exemplarily, the positive current collector includes but is not limited to at least one of aluminum foil, carbon-coated aluminum foil, iron foil, tin foil, zinc foil, nickel foil, titanium foil, and manganese foil. Exemplarily, the conductive agent includes but is not limited to one or more of graphite, carbon black, acetylene black, graphene, carbon fiber, C60, and carbon nanotubes, and the content of the conductive agent in the positive active layer is 3wt% to 5wt%. Exemplarily, the binder includes but is not limited to one or more of polyvinylidene chloride, soluble polytetrafluoroethylene, styrene-butadiene rubber, hydroxypropyl methylcellulose, methylcellulose, carboxymethyl cellulose, polyvinyl alcohol, acrylonitrile copolymer, sodium alginate, chitosan, and chitosan derivatives, and the content of the binder in the positive active layer is 2wt% to 4wt%.
[0154] In some embodiments, the preparation process of the positive electrode plate can be: mixing the positive electrode active material, the conductive agent, the binder and the lithium supplement agent to obtain an electrode slurry, coating the electrode slurry on the positive electrode collector, and preparing the positive electrode plate through drying, rolling, die cutting and other steps, wherein the lithium supplement agent includes the composite lithium supplement material of the present application.
[0155] The catalyst, composite lithium supplement material, preparation method and application thereof of the present application are illustrated by multiple specific embodiments below.
[0156] Composite catalyst, composite lithium supplement material and preparation method thereof:
[0157] Example 1
[0158] This embodiment provides a composite catalyst and a composite lithium supplement material.
[0159] The composite lithium supplement material includes a composite catalyst and a lithium-rich material (lithium oxalate). The composite catalyst includes a sulfur-doped biomass carbon material and a transition metal compound uniformly distributed in the biomass carbon material. The lithium-rich material is uniformly distributed in the composite catalyst. Specifically: the biomass carbon material has a porous structure, part of the transition metal compound and part of the lithium-rich material are independently attached to the outer surface of the biomass carbon material, part of the transition metal compound and part of the lithium-rich material are independently distributed in the pores of the biomass carbon material, and part of the lithium-rich material is in contact with the transition metal compound. Transition metal compounds include MoS2, Co3S4 and Fe 0.92 Co 0.08 A PP heterostructure is formed between S, MoS2 and Co3S4. The mass ratio of lithium-rich material, transition metal compound and biomass carbon material is 60:26:13, the D50 particle size of transition metal compound is 500nm, and the D50 particle size of lithium-rich material is 600nm.
[0160] The preparation method of the composite catalyst and the composite lithium supplement material comprises the following steps:
[0161] Step S1, add 3mmol FeCl2·4H2O and 3mmol Co(NO3)2·6H2O into 100mL deionized water to dissolve, then add 0.1g original poplar fiber, soak at room temperature (20°C) for 24h, filter, and obtain a pretreated carbon source.
[0162] Step S2, 0.2 mmol 2,5-dihydroxyterephthalic acid (DOBDC), 2 mmol FeCl2·4H2O and 1 mmol Co(NO3)2·6H2O were respectively added into 100 mL of a mixed solvent (dimethylformamide, ethanol and deionized water in a volume ratio of 10:2:1) to form a raw material solution.
[0163] Step S3, adding 0.1 g of pretreated carbon source to the raw material liquid, transferring to a hydrothermal reactor, hydrothermally reacting at 120° C. for 24 h, cooling to room temperature after the reaction, washing with anhydrous ethanol, and vacuum drying at 60° C. for 12 h to obtain a catalyst precursor, recorded as MOF-74-FeCo / WF.
[0164] Step S4, adding 1g MOF-74-FeCo / WF, 0.5g sodium molybdate dihydrate and 4g thioacetamide to 50mL ethanol, transferring the solution to an autoclave for sulfidation reaction after it is completely dissolved, and the sulfidation reaction conditions are: reacting at 120°C for 4h, then reacting at 200°C for 8h, collecting the precipitate after cooling, washing 4 times, and then drying at 60°C for 8h to obtain a catalyst intermediate, recorded as MoS2@Co3S4@MOF-74-FeCo / WF.
[0165] Step S5: 0.3 g of the catalyst intermediate and 1 g of sulfur powder are placed in corundum boats, which are then placed in the center and upstream of a tube furnace for calcination at 2 °C / min. -1 The tube furnace was heated from room temperature to 300 °C at a heating rate, kept at 300 °C for 2 h, then heated to 500 °C, kept for 2 h, and finally kept at 700 °C for 4 h under nitrogen atmosphere to obtain the catalyst, which was recorded as MoS2@Co3S4@Fe 0.92 Co 0.08 S / SCWF.
[0166] Step S6, add 0.1 g of the catalyst to 50 mL of a saturated aqueous solution of lithium oxalate, disperse by ultrasonic, then add ethanol, collect the precipitate by filtration, and dry to obtain a composite lithium supplement material, recorded as MoS2@Co3S4@Fe 0.92 Co 0.08 S / SCWF@Li2C2O4.
[0167] Example 2
[0168] This embodiment provides a composite catalyst and a composite lithium supplement material, which differ from the embodiment 1 in that: in the composite catalyst, the distribution form of the transition metal compound is different, specifically: in the composite catalyst, the transition metal compound is only attached to the outer surface of the biomass carbon material. In the composite lithium supplement material, the mass ratio of the lithium-rich material, the transition metal compound and the biomass carbon material is 60:16:13, the D50 particle size of the transition metal compound is 500nm, the D50 particle size of the lithium-rich material is 600nm, and the rest is the same as the embodiment 1.
[0169] The preparation method of the composite catalyst and the composite lithium supplement material is different from that of Example 1 in that the amount of the pretreated carbon source added in step S3 is 1 g, and the rest is the same as that of Example 1.
[0170] Example 3
[0171] This embodiment provides a composite catalyst and a composite lithium-supplementing material, which differ from Embodiment 1 in that: in the composite catalyst, the distribution form of the transition metal compound is different, specifically: in the composite catalyst, the transition metal compound is attached to the outer surface of the biomass carbon material, at least part of the transition metal compound is continuously coated on the outer surface of the biomass carbon material, and part of the transition metal compound is filled in the pores of the biomass carbon material; in the composite lithium-supplementing material, the mass ratio of the lithium-rich material, the transition metal compound and the biomass carbon material is 60:50:13, the D50 particle size of the transition metal compound is 500nm, and the D50 particle size of the lithium-rich material is 600nm, and the rest is the same as Embodiment 1.
[0172] The preparation method of the composite catalyst and the composite lithium supplement material is different from that of Example 1 in that the added amounts of DOBDC, FeCl2·4H2O and Co(NO3)2·6H2O in step S2 are different, specifically:
[0173] Step S2, 2 mmol 2,5-dihydroxyterephthalic acid (DOBDC), 20 mmol FeCl2·4H2O and 10 mmol Co(NO3)2·6H2O were respectively added into 100 mL of a mixed solvent (dimethylformamide, ethanol and deionized water in a volume ratio of 10:2:1) to form a raw material solution.
[0174] Example 4
[0175] This embodiment provides a composite catalyst and a composite lithium-supplementing material, which differ from Embodiment 1 in that: in the composite lithium-supplementing material, the distribution form of the lithium-rich material is different, specifically: the lithium-rich material is only attached to the outer surface of the biomass carbon material, wherein the mass ratio of the lithium-rich material, the transition metal compound and the biomass carbon material is 40:26:13, the D50 particle size of the transition metal compound is 500nm, the D50 particle size of the lithium-rich material is 600nm, and the rest is the same as Embodiment 1.
[0176] The method for preparing the composite catalyst and the composite lithium-rich material is different from that of Example 1 in that in step S6, the volume of the saturated aqueous solution of lithium oxalate is 10 mL.
[0177] Example 5
[0178] This embodiment provides a composite catalyst and a composite lithium-supplementing material, which differ from Embodiment 1 in that: in the composite lithium-supplementing material, the distribution form of the lithium-rich material is different, specifically: the lithium-rich material is attached to the outer surface of the biomass carbon material, at least part of the lithium-rich material is continuously coated on the outer surface of the biomass carbon material, and part of the lithium-rich material is filled in the pores of the biomass carbon material, wherein the mass ratio of the lithium-rich material, the transition metal compound and the biomass carbon material is 70:26:13, the D50 particle size of the transition metal compound is 500nm, the D50 particle size of the lithium-rich material is 600nm, and the rest is the same as Embodiment 1.
[0179] The method for preparing the composite catalyst and the composite lithium-rich material is different from that of Example 1 in that in step S6, the volume of the saturated aqueous solution of lithium oxalate is 100 mL.
[0180] Example 6
[0181] This embodiment provides a composite catalyst and a composite lithium supplement material, which are different from the embodiment 1 in that the particle size of the transition metal compound is different, wherein the D50 particle size of the transition metal compound is 700 nm, and the rest is the same as the embodiment 1.
[0182] The preparation method of the composite catalyst and composite lithium-rich material is different from that of Example 1 in that the conditions for the hydrothermal reaction in step S3 are: 200°C / 24h, and the conditions for the sulfidation reaction in step S4 are: reacting at 140°C for 4h and then reacting at 220°C for 8h.
[0183] Example 7
[0184] This embodiment provides a composite catalyst and a composite lithium supplement material, which differs from the embodiment 1 in that the types of transition metal compounds are different, specifically, the transition metal compounds include MoSe2, Co3Se4 and Fe 0.92 Co 0.08 A PP heterostructure is formed between Se, MoSe2 and Co3Se4.
[0185] The preparation method of the composite catalyst and the composite lithium-rich material is different from that of Example 1 in that:
[0186] The thioacetamide in step S4 is replaced by selenoamide, and the sulfur powder in step S5 is replaced by selenium powder.
[0187] Example 8
[0188] This embodiment provides a composite catalyst and a composite lithium-supplementing material, which differs from Embodiment 1 in that the biomass carbon material is not doped with sulfur, and the transition metal compound only includes MoS2 and Co3S4, wherein the mass ratio of the lithium-rich material, the transition metal compound and the biomass carbon material is 60:26:13, the D50 particle size of the transition metal compound is 500nm, the D50 particle size of the lithium-rich material is 600nm, and the rest is the same as Embodiment 1.
[0189] The preparation method of the composite catalyst and the composite lithium-rich material is different from that of Example 1 in that in step S5, only the catalyst intermediate is used for calcination treatment, specifically:
[0190] Step S5: 0.3 g of the catalyst intermediate was placed in a corundum boat, placed in the center of a tube furnace, and heated at 2 °C / min. -1 The tubular furnace was heated from room temperature to 300°C at a heating rate, maintained at 300°C for 2 h, then heated to 500°C, maintained for 2 h, and finally maintained at 700°C for 4 h under a nitrogen atmosphere to obtain the catalyst, which was recorded as MoS2@Co3S4 / CWF.
[0191] Example 9
[0192] This embodiment provides a catalyst and a composite lithium supplement material, which differs from Embodiment 1 in that lithium oxalate is replaced by lithium squarate, and the rest is the same as Embodiment 1.
[0193] Example 10
[0194] This comparative example provides a composite lithium supplement material, which is different from Example 1 in that there is no heterogeneous structure between the transition metal compounds. The mass ratio of the lithium-rich material, the transition metal compound and the biomass carbon material is 60:26:13, the D50 particle size of the transition metal compound is 500nm, and the D50 particle size of the lithium-rich material is 600nm.
[0195] The method for preparing the catalyst and the composite lithium supplement material is different from that of Example 1 in that step S4 is deleted, and the catalyst intermediate in step S5 is replaced by the catalyst precursor in step S3.
[0196] Comparative Example 1
[0197] This comparative example provides a composite lithium supplement material, which includes lithium oxalate and a transition metal compound in a mass ratio of 60:26, wherein the transition metal compound and the lithium oxalate are simply mixed, wherein the transition metal compound includes MoS2, Co3S4 and Fe 0.92 Co 0.08 S.
[0198] Comparative Example 2
[0199] This comparative example provides a lithium supplement material, which only includes lithium oxalate.
[0200] Comparative Example 3
[0201] This comparative example provides a lithium supplement material, which only includes lithium squarate.
[0202] Lithium-ion battery example:
[0203] The composite lithium supplement materials provided in Examples 1 to 10 and the lithium supplement materials provided in Comparative Examples 1 to 3 are respectively assembled into positive electrodes and lithium ion batteries according to the following methods:
[0204] Positive electrode: Under the same conditions, the composite lithium supplement material: SP (conductive carbon black): PVDF (polyvinylidene fluoride) are mixed in a mass ratio of 90:4:6, and N-methylpyrrolidone (NMP) is used as a solvent to mix the materials evenly to form a slurry, which is then evenly coated on the surface of the aluminum foil, rolled to a certain thickness, and vacuum dried at 110°C for 12 hours to form a positive electrode sheet; wherein the composite lithium supplement material is the composite lithium supplement material provided in the above-mentioned Examples 1 to 10 and the lithium supplement material provided in the comparative example.
[0205] Counter electrode: lithium metal sheet.
[0206] Electrolyte: The electrolyte is a 1 mol / L LiPF6 / ethylene carbonate:ethyl methyl carbonate (volume ratio) = 1:1 solution.
[0207] Diaphragm: Polypropylene microporous membrane.
[0208] Lithium-ion battery assembly: The lithium metal sheet-diaphragm-electrolyte-positive electrode sheet assembly sequence is assembled into a button-type lithium-ion battery in an inert atmosphere glove box. The batteries containing the composite lithium supplement materials provided in Examples 1 to 10 are respectively recorded as Examples S1 to S10, and the batteries containing the lithium supplement materials provided in Comparative Examples 1 to 3 are recorded as Comparative Examples DS1 to DS3.
[0209] Performance Testing
[0210] (1) AC impedance test
[0211] The assembled button cell was subjected to an alternating current impedance test using an electrochemical workstation to obtain the EIS spectra of the lithium supplement additives in each embodiment and comparative example, and corresponding fitting was performed to obtain the charge transfer resistance (Rct) of each lithium supplement additive.
[0212] (2) Electrochemical performance test
[0213] The electrochemical performance of each lithium ion battery assembled in the above lithium ion battery embodiment was tested as shown in Table 1, and the test conditions were as follows:
[0214] The battery was charged at a rate of 0.1C with a cut-off voltage of 4.7V; constant voltage charging was performed at a cut-off voltage of 4.7V; after the charging process was completed, the battery was allowed to stand for 10 minutes and then discharged at a rate of 0.1C with a cut-off voltage of 2.5V; the charging platform was observed during the charging process to obtain the delithiation potential of the composite lithium supplement material.
[0215] The relevant performance test results of the composite lithium supplement material and lithium secondary battery are shown in Table 1 below.
[0216] Table 1 Related performance test results
[0217]
[0218]
[0219] Result analysis:
[0220] It can be seen from Table 1 that the delithiation potential and charge transfer resistance of the composite lithium-supplementing materials in the lithium batteries prepared in Examples S1-S10 of the present application are lower than those in Comparative Examples DS1-DS3, which indicates that the composite catalyst formed by the biomass carbon material combined with the transition metal compound can improve the conductivity of the lithium-rich material, thereby effectively reducing the delithiation potential of the lithium-rich material.
[0221] It can be seen from Examples 1-3 that an appropriate proportion of transition metal compounds can effectively improve the electrochemical properties of composite lithium supplement materials, and specifically, the electrochemical properties of Example S1 are better. The reason is that transition metal compounds can catalyze lithium oxalate, thereby reducing its delithiation potential, and there are heterogeneous structures in transition metal compounds. In addition, the presence of biomass carbon materials is more conducive to improving the conductivity of lithium-rich materials, thereby achieving a better lithium supplement effect. However, since transition metal compounds cannot provide active ions, although the charge transfer resistance and delithiation potential are low in Example S3, its first charge capacity is lower than that in Example S1.
[0222] Combining Examples S1, S4-S5, it can be seen that the electrochemical performance of Example S1 is more advantageous. The reason is that the ratio of lithium-rich materials, transition metal compounds and biomass carbon materials in Example 1 is relatively appropriate, which can achieve full contact between lithium oxalate and transition metal compounds and biomass carbon materials, thereby giving full play to the lithium supplement performance of the composite lithium supplement material. The composite lithium supplement material synthesized in Example 4 contains less lithium oxalate, and its first charging capacity is not advantageous. The composite lithium supplement material synthesized in Example 5 contains more lithium oxalate, and the lithium oxalate is also continuously coated on the outer surface of the biomass carbon material. In this case, the composite catalyst cannot catalyze the delithiation of a large amount of lithium oxalate.
[0223] Combining Examples S1 and S6, it can be seen that the appropriate size of the transition metal compound is more conducive to the delithiation of lithium oxalate. The reason is that the particle size of the transition metal compound in Example 6 is large, which further affects the contact effect between lithium oxalate and the transition metal compound.
[0224] It can be seen from Examples S1 and S7 that a variety of transition metal compounds are suitable for this system, and can improve the conductivity of lithium oxalate and effectively reduce the delithiation potential of lithium oxalate.
[0225] It can be seen from Examples S1 and S9 that the composite catalyst formed by combining biomass carbon materials with transition metal compounds can be used to catalyze a variety of lithium-rich materials with a voltage above 4V, such as lithium oxalate, lithium squarate, etc., which can improve their conductivity and effectively reduce their delithiation potential.
[0226] Combining Examples S1, S8, and S10, it can be seen that the doped sulfur element in the biomass carbon material and the heterogeneous structure in the transition metal compound in Example 1 can significantly improve the electrical conductivity of the material and reduce its delithiation potential. The reason is that sulfur doping can change the electronic structure and surface polarity of the biomass carbon material, thereby effectively improving the electrical conductivity and catalytic activity of the composite catalyst; the presence of the heterogeneous structure can form a special electron transfer path at the heterojunction interface to promote electron transfer, thereby further promoting the decomposition of lithium oxalate, making the decomposition voltage of lithium oxalate drop more significantly.
[0227] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A composite catalyst, characterized in that: It comprises a biomass carbon material and a transition metal compound, wherein the transition metal compound is uniformly distributed in the biomass carbon material.
2. The composite catalyst according to claim 1, characterized in that The biomass carbon material has a porous structure, and the transition metal compound is distributed in the porous structure of the biomass carbon material and / or on the surface of the biomass carbon material; and / or, The biomass carbon material is doped with at least one non-metallic element of S, N, and P; and / or, The transition metal compound contains at least two different transition metal compounds, and a heterojunction is formed between the two transition metal compounds.
3. The composite catalyst according to claim 1, characterized in that The loading amount of the transition metal compound in the biomass carbon material is 80%-400%; and / or, The density of the composite catalyst is 6.4 g / cm 3 -10g / cm 3 , the density standard deviation of the composite catalyst is 0.6-0.9; and / or, The D50 particle size of the transition metal compound is 50nm-1000nm; and / or, The specific surface area of the biomass carbon material is 10m 2 / g-500m 2 / g; and / or, The biomass carbon material has a diameter of 0.6 μm-10 μm and a length of 10 μm-40 μm.
4. A composite lithium supplement material, characterized in that: include: Lithium-rich materials, and The composite catalyst according to any one of claims 1 to 3, wherein the composite catalyst is combined with the lithium-rich material.
5. The composite lithium supplement material according to claim 4, characterized in that: The lithium-rich material is uniformly distributed in the composite catalyst.
6. The composite lithium supplement material according to claim 4, characterized in that: The biomass carbon material includes one or more of a rod-shaped, a fiber-shaped, a cylindrical and a spindle-shaped; and / or, Part of the lithium-rich material is attached to the transition metal compound; and / or, The biomass carbon material has a porous structure, and part of the lithium-rich material is distributed in the porous structure of the biomass carbon material and / or on the surface of the biomass carbon material.
7. The composite lithium supplement material according to any one of claims 4 to 6, characterized in that: The mass ratio of the lithium-rich material to the transition metal compound in the composite catalyst and the biomass carbon material is 40-90:5-50:5-20; and / or, The D50 particle size of the lithium-rich material is 100nm-1000nm; and / or, The lithium-rich material includes an organic lithium salt.
8. A method for preparing a composite lithium supplement material, characterized in that: The following steps are involved: The biomass carbon source, the first metal source, and the organic matter are mixed in a solution system, and subjected to hydrothermal treatment, so that the metal ions in the first metal source coordinate with the organic matter to form a metal organic framework and combine with the biomass carbon source to obtain a catalyst precursor; The catalyst precursor, the second metal source and the first reaction source are reacted in a solution system to obtain a catalyst intermediate; The catalyst intermediate and the second reaction source are mixed and calcined to obtain a composite catalyst; The composite catalyst and the lithium-rich material are mixed to obtain a composite lithium-supplementing material.
9. A positive electrode, characterized in that The invention comprises a positive electrode active material and a lithium supplement material, wherein the lithium supplement material comprises the composite lithium supplement material according to any one of claims 4 to 7 and / or the composite lithium supplement material prepared by the preparation method of the composite lithium supplement material according to claim 8.
10. A secondary battery, comprising a positive electrode sheet, a negative electrode sheet and an electrolyte, characterized in that: The positive electrode sheet comprises the positive electrode according to claim 9.