Electrolyte diaphragm and preparation method thereof
By using the cluster electrolyte generated by the complex reaction of lithium salt and organic solvent in the lithium-ion battery separator, combining performance optimizer and flame retardant, the problem of lithium battery separator is solved, and the battery is realized high energy density and low cost production.
Patent Information
- Application Number
- CN202411243865.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-19
AI Technical Summary
Existing lithium-ion battery separators are flammable and explosive under high temperature or abuse, and the production cost of solid electrolyte separators is high, making it difficult to meet the thermal stability and economic requirements of lithium batteries.
The cluster electrolyte generated by the complexation reaction of lithium salt and organic solvent is used to combine performance optimization agents and flame retardants to form an electrolyte membrane uniformly dispersed in the separator matrix, and through simple preparation methods such as heating or electrospinning Technical preparation.
It realizes good thermal stability and low production cost of electrolyte separators, improves the room temperature ionic conductivity and electrochemical window of lithium batteries, is suitable for high-voltage battery systems, and reduces the production cost of lithium batteries.
Smart Images

Figure BDA0005030041420000191
Abstract
Description
Technical Field
[0001] The present application relates to the field of lithium batteries, and in particular to an electrolyte membrane and a preparation method thereof. Background Art
[0002] As a carrier of energy storage, lithium-ion batteries have the advantages of high energy density, long cycle life, small self-discharge effect, and environmental friendliness. They have been widely used in portable electronic products such as mobile phones, laptops, and power tools, and are gradually becoming dominant in the fields of transportation and large-scale energy storage. As an important component of lithium-ion batteries, the separator plays a vital role inside lithium-ion batteries.
[0003] In conventional liquid lithium batteries, the separator plays the role of isolating the positive and negative electrode materials of the battery to prevent internal short circuits and provide a channel for the migration of lithium ions. However, it does not have ion conductivity itself and needs to be combined with liquid electrolyte to realize ion transport within the battery.
[0004] In order to make the separator match more battery forms, for example, solid-state batteries, an electrolyte separator has been developed that can isolate the positive and negative electrode materials of the battery to prevent internal short circuits and has ion conductivity. Generally, the electrolyte separator can be divided into a gel electrolyte separator and a solid electrolyte separator.
[0005] Gel electrolyte separators are usually composed of a base membrane material and a liquid organic electrolyte, and rely on the liquid organic electrolyte adsorbed in the base membrane material to achieve ionic conductivity. However, liquid organic electrolytes are flammable and easy to vaporize, and under abuse such as high temperature and needle puncture, the battery will catch fire due to thermal runaway.
[0006] Solid electrolyte separators usually contain or consist of oxide solid electrolytes, sulfide solid electrolytes or polymer solid electrolytes. Solid electrolytes are safer than liquid electrolytes, but they are expensive and difficult to produce. Their large-scale application significantly increases the production cost of batteries.
[0007] Therefore, it is necessary to develop an electrolyte membrane with good thermal stability and low production cost. Summary of the invention
[0008] The purpose of the present application is to provide an electrolyte membrane having good thermal stability and low production cost.
[0009] In a first aspect, the present application provides an electrolyte membrane, comprising a membrane matrix and a cluster electrolyte uniformly dispersed in the membrane matrix, wherein the cluster electrolyte comprises complex molecules generated by complex reaction of cations of a lithium salt with organic solvent molecules, and anions of the lithium salt located in the solvation sheath of the cations, and the organic solvent comprises at least one of a carbonate solvent, a fluorocarbonate solvent, an ether solvent, a fluoroether solvent, a carboxylate solvent, a sulfite solvent, a phosphate solvent and a sulfone solvent.
[0010] In some embodiments, the lithium salt includes at least one of lithium trifluoromethylsulfonate, lithium bistrifluoromethylsulfonyl imide, lithium bisfluorosulfonyl imide, lithium di(polyfluoroalkylsulfonyl)imide, lithium di(polyfluoroalkoxysulfonyl)imide, tri(trifluoromethylsulfonyl)methyl lithium, lithium bisoxalatoborate, and lithium difluorooxalatoborate.
[0011] In some embodiments, the material of the membrane matrix includes at least one of polyolefin, polyimide, cellulose, polyacrylonitrile, polyurethane, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyacrylate and polylactic acid.
[0012] In some embodiments, the electrolyte membrane further comprises a performance optimizer and / or a flame retardant; the performance optimizer comprises vinylene carbonate, vinyl ethylene carbonate, ethylene sulfate, ethylene sulfite, propylene sulfate, propylene sulfite, 4-methylethylene sulfate, 4-methylethylene sulfite, 1,4-butane sultone, 1,3-propane sultone, cyclohexylbenzene, tris(trimethylsilane) phosphate, tris(trimethylsilane) phosphite, tris(trimethylsilane) borate, succinonitrile, adiponitrile, pentafluoropropionic anhydride, fluoroethylene carbonate, difluoroboron oxalate The flame retardant comprises at least one of lithium phosphate, lithium bis(trifluoromethanesulfonyl imide), lithium bis(fluorosulfonyl imide), lithium tetrafluoroborate, lithium bis(oxalatoborate), lithium difluorophosphate and lithium nitrate; the flame retardant comprises at least one of tris(2,2,2-trifluoroethyl)phosphite, tris(4-fluorophenyl)phosphine, tris(2,2,3,3,3-pentafluoropropyl)phosphate, triphenyl phosphite, trimethyl phosphite, triethyl phosphite, tributyl phosphite, dimethyl methylphosphonate, diethyl ethylphosphonate, ethoxy pentafluorocyclotriphosphazene, phenoxy pentafluorocyclotriphosphazene, hexamethoxycyclotriphosphazene and ionic liquid.
[0013] In a second aspect, the present application also provides a method for preparing an electrolyte membrane, comprising: providing a membrane matrix raw material, the membrane matrix raw material comprising a high molecular weight polymer and a first organic solvent, the high molecular weight polymer being dissolved in the first organic solvent; providing a cluster electrolyte precursor, the cluster electrolyte precursor comprising a lithium salt and a second organic solvent, the lithium salt being dissolved in the second organic solvent; and mixing the cluster electrolyte precursor with the membrane matrix raw material, causing the first organic solvent in the membrane matrix raw material to volatilize to form a membrane matrix, causing the molecules of the second organic solvent in the cluster electrolyte precursor to volatilize to form a membrane matrix, and causing the molecules of the second organic solvent in the cluster electrolyte precursor to volatilize to form a membrane matrix. The lithium salt combines to form a cluster electrolyte, and the second organic solvent that has not formed the cluster electrolyte is volatilized to form the electrolyte membrane; wherein the cluster electrolyte includes complex molecules generated by the complex reaction of the cations of the lithium salt and the molecules of the second organic solvent, and the anions of the lithium salt located in the solvation sheath of the cations, and the cluster electrolyte is uniformly dispersed in the membrane matrix; the second organic solvent includes at least one of carbonate solvents, fluorocarbonate solvents, ether solvents, fluoroether solvents, carboxylate solvents, sulfite solvents, phosphate solvents and sulfone solvents.
[0014] In some embodiments, the lithium salt includes at least one of lithium trifluoromethylsulfonate, lithium bistrifluoromethylsulfonyl imide, lithium bisfluorosulfonyl imide, lithium di(polyfluoroalkylsulfonyl)imide, lithium di(polyfluoroalkoxysulfonyl)imide, tri(trifluoromethylsulfonyl)methyl lithium, lithium bisoxalatoborate, and lithium difluorooxalatoborate.
[0015] In some embodiments, the high molecular polymer includes at least one of polyacrylonitrile, polyurethane, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyacrylate and polylactic acid; and / or the first organic solvent includes at least one of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, acetone, tetrahydrofuran, acetonitrile, ethyl acetate, toluene and xylene.
[0016] In some embodiments, the cluster electrolyte precursor further includes at least one of a performance optimizer and a flame retardant; the performance optimizer includes vinyl carbonate, vinyl ethylene carbonate, ethylene sulfate, ethylene sulfite, propylene sulfate, propylene sulfite, 4-methylethylene sulfate, 4-methylethylene sulfite, 1,4-butane sultone, 1,3-propane sultone, cyclohexylbenzene, tris(trimethylsilane) phosphate, tris(trimethylsilane) phosphite, tris(trimethylsilane) borate, succinonitrile, adiponitrile, pentafluoropropionic anhydride, fluoroethylene carbonate, difluoro At least one of lithium oxalatoborate, lithium bistrifluoromethanesulfonyl imide, lithium bisfluorosulfonyl imide, lithium tetrafluoroborate, lithium bisoxalatoborate, lithium difluorophosphate and lithium nitrate; and the flame retardant includes at least one of tris(2,2,2-trifluoroethyl)phosphite, tris(4-fluorophenyl)phosphine, tris(2,2,3,3,3-pentafluoropropyl)phosphate, triphenyl phosphite, trimethyl phosphite, triethyl phosphite, tributyl phosphite, dimethyl methylphosphonate, diethyl ethylphosphonate, ethoxypentafluorocyclotriphosphazene, phenoxypentafluorocyclotriphosphazene, hexamethoxycyclotriphosphazene and ionic liquid.
[0017] In some embodiments, the cluster electrolyte precursor is mixed with the diaphragm matrix raw material, the first organic solvent in the diaphragm matrix raw material is volatilized to form a diaphragm matrix, the molecules of the second organic solvent in the cluster electrolyte precursor are combined with the lithium salt to form a cluster electrolyte, and the second organic solvent that has not formed the cluster electrolyte is volatilized. The method for forming the electrolyte diaphragm includes: mixing the cluster electrolyte precursor with the diaphragm matrix raw material to obtain a mixed liquid; and applying the mixed liquid to the surface of a film-forming substrate, and heating and / or applying negative pressure to the mixed liquid applied to the surface of the film-forming substrate, so that the first organic solvent in the diaphragm matrix raw material is volatilized to form a diaphragm matrix, the molecules of the second organic solvent in the cluster electrolyte precursor are combined with the lithium salt to form a cluster electrolyte, and the second organic solvent that has not formed the cluster electrolyte is volatilized to form the electrolyte diaphragm.
[0018] In some embodiments, the cluster electrolyte precursor is mixed with the diaphragm matrix raw material, the first organic solvent in the diaphragm matrix raw material is volatilized to form a diaphragm matrix, the molecules of the second organic solvent in the cluster electrolyte precursor are combined with the lithium salt to form a cluster electrolyte, and the second organic solvent that has not formed the cluster electrolyte is volatilized. The method for forming the electrolyte diaphragm includes: mixing the cluster electrolyte precursor with the diaphragm matrix raw material to obtain a mixed liquid; and using the mixed liquid for electrospinning, the first organic solvent in the diaphragm matrix raw material is volatilized to form a diaphragm matrix, the molecules of the second organic solvent in the cluster electrolyte precursor are combined with the lithium salt to form a cluster electrolyte, and the second organic solvent that has not formed the cluster electrolyte is volatilized to form the electrolyte diaphragm.
[0019] The beneficial effects of the electrolyte membrane and the preparation method thereof provided in the present application include but are not limited to the following:
[0020] The electrolyte membrane provided in the present application has good room temperature ionic conductivity and a wider electrochemical window (the electrochemical window of liquid and gel electrolytes is usually ≤4.5V). Therefore, the electrolyte membrane provided in the present application can be applied to battery systems with high-voltage positive electrode materials, which can enable lithium batteries to have higher energy density.
[0021] In addition, the electrolyte membrane provided by the present application does not contain liquid organic electrolyte, so its thermal stability is better than that of gel electrolyte membrane. The electrolyte membrane provided by the present application does not require the use of higher-cost solid electrolytes such as oxide solid electrolytes, sulfide solid electrolytes or polymer solid electrolytes during the preparation process, so its production cost is lower than that of solid electrolyte membrane.
[0022] In addition, the production process of the electrolyte membrane provided in the present application is simple, has the potential for large-scale application, and has important application value for the development of high-energy-density and high-safety lithium batteries. DETAILED DESCRIPTION
[0023] The following description provides specific application scenarios and requirements of the present application, with the purpose of enabling those skilled in the art to make and use the content in the present application. It will be apparent to those skilled in the art that various local modifications to the disclosed embodiments are apparent, and the general principles defined herein may be applied to other embodiments and applications without departing from the spirit and scope of the present application. Therefore, the present application is not limited to the embodiments shown, but to the widest scope consistent with the claims.
[0024] In a first aspect, the present application provides an electrolyte membrane, comprising a membrane matrix and a cluster electrolyte uniformly dispersed in the membrane matrix, wherein the cluster electrolyte comprises complex molecules generated by complex reaction of cations of a lithium salt with organic solvent molecules, and anions of the lithium salt located in the solvation sheath of the cations.
[0025] The cluster electrolyte includes complex molecules generated by complex reaction between the cations of the lithium salt and the molecules of the second organic solvent, and anions of the lithium salt located in the solvation sheath of the cations, and the cluster electrolyte is uniformly dispersed in the diaphragm matrix. The solvation sheath described in this application refers to a layer of solvent molecules surrounding the lithium salt cations, i.e., lithium ions, and the organic solvent molecules are tightly combined with the lithium ions through complexation to form a solvation sheath.
[0026] The cluster electrolyte is a complexation between the cations of the lithium salt and the molecules of the organic solvent, and at the same time, the anions of the lithium salt enter the solvation sheath of the lithium salt cations under the Coulomb force between the cations of the lithium salt, so that the "lithium salt cations-organic solvent molecules-lithium salt anions" are "bound" together to form a cluster electrolyte. The conductive mechanism of the cluster electrolyte is that under the action of the electric field, the lithium ions in the cluster migrate from one lithium salt anion to another lithium salt anion with the assistance of the solvation sheath, thereby achieving ion conduction.
[0027] The organic solvent includes at least one of a carbonate solvent, a fluorocarbon solvent, an ether solvent, a fluoroether solvent, a carboxylate solvent, a sulfite solvent, a phosphate solvent and a sulfone solvent.
[0028] In some embodiments, the carbonate solvent includes at least one of ethylene carbonate, 1,2-dimethylethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, dibutyl carbonate and derivatives thereof.
[0029] In some embodiments, the fluorocarbonate solvent includes at least one of fluoroethylene carbonate, bisfluoroethylene carbonate, trifluoromethylethylene carbonate, methyl trifluoroethyl carbonate, fluorodimethyl carbonate and derivatives thereof.
[0030] In some embodiments, the ether solvent includes at least one of tetrahydrofuran, dioxolane, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol dibutyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether and derivatives thereof.
[0031] In some embodiments, the fluoroether solvent is a linear fluoroether with the structural formula: R1 -OR 2 , where R 1 and R 2 It may be methyl, ethyl, propyl, isopropyl, butyl, sec-butyl, isobutyl, tert-butyl, pentyl, isopentyl, etc., or a group in which some or all of the hydrogen atoms are substituted with fluorine.
[0032] In some embodiments, the fluoroether solvent includes at least one of 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, 1,1,2,3,3,3-hexafluoropropyl-2,2,2-trifluoroethyl ether, 1,1,1,3,3,3-hexafluoropropyl-methyl ether, 1,1,1,2,3,3-hexafluoropropyl-2,2,3,3-tetrafluoropropyl ether and 1H,1H,5H-octafluoropentyl-1,1,2,2-tetrafluoroethyl ether.
[0033] In some embodiments, the carboxylate solvent includes at least one of methyl formate, methyl acetate, and ethyl acetate.
[0034] In some embodiments, the sulfite solvent includes at least one of dimethyl sulfite and diethyl sulfite.
[0035] In some embodiments, the phosphate ester solvent includes at least one of trimethyl phosphate, triethyl phosphate, tributyl phosphate, trioctyl phosphate, triphenyl phosphate, ethylene ethyl phosphate, and tris(2,2,2-trifluoroethyl) phosphate.
[0036] In some embodiments, the sulfone solvent includes at least one of dimethyl sulfoxide and sulfolane.
[0037] In some embodiments, the lithium salt includes at least one of lithium trifluoromethylsulfonate, lithium bistrifluoromethylsulfonyl imide, lithium bisfluorosulfonyl imide, lithium di(polyfluoroalkylsulfonyl)imide, lithium di(polyfluoroalkoxysulfonyl)imide, tri(trifluoromethylsulfonyl)methyl lithium, lithium bisoxalatoborate, and lithium difluorooxalatoborate.
[0038] The lithium salt is an organic electrolyte lithium salt that can be used in lithium battery electrolytes, and the organic solvent is a solvent that can be used in lithium battery electrolytes, which makes the production cost of the cluster electrolyte similar to that of conventional lithium battery electrolytes, and the production process is simple and easy to control.
[0039] In some embodiments, the material of the membrane matrix includes at least one of polyolefin, polyimide, cellulose, polyacrylonitrile, polyurethane, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyacrylate and polylactic acid.
[0040] In some embodiments, the electrolyte membrane further includes a performance optimizer and / or a flame retardant.
[0041] The performance optimizer is used to improve the ionic conductivity, electrochemical window and long cycle stability of the cluster electrolyte. In some embodiments, the performance optimizer includes vinylene carbonate, vinyl ethylene carbonate, ethylene sulfate, ethylene sulfite, propylene sulfate, propylene sulfite, 4-methylethylene sulfate, 4-methylethylene sulfite, 1,4-butane sultone, 1,3-propane sultone, cyclohexylbenzene, tris(trimethylsilane) phosphate, tris(trimethylsilane) phosphite, tris(trimethylsilane) borate, succinonitrile, adiponitrile, pentafluoropropionic anhydride, fluoroethylene carbonate, difluorooxalato lithium borate, bistrifluoromethanesulfonyl imide lithium, bisfluorosulfonyl imide lithium, lithium tetrafluoroborate, lithium bisoxalato borate, lithium difluorophosphate and lithium nitrate.
[0042] Since the cluster electrolyte may burn under extreme abuse conditions, adding the flame retardant can further improve the intrinsic safety of the cluster electrolyte. In some embodiments, the flame retardant includes at least one of tris(2,2,2-trifluoroethyl)phosphite, tris(4-fluorophenyl)phosphine, tris(2,2,3,3,3-pentafluoropropyl)phosphate, triphenyl phosphite, trimethyl phosphite, triethyl phosphite, tributyl phosphite, dimethyl methylphosphonate, diethyl ethylphosphonate, ethoxy pentafluorocyclotriphosphazene, phenoxy pentafluorocyclotriphosphazene, hexamethoxycyclotriphosphazene and ionic liquid.
[0043] In the second aspect, the present application also provides a method for preparing an electrolyte diaphragm, comprising: providing a diaphragm matrix raw material, the diaphragm matrix raw material comprising a polymer and a first organic solvent, the polymer being dissolved in the first organic solvent; providing a cluster electrolyte precursor, the cluster electrolyte precursor comprising a lithium salt and a second organic solvent, the lithium salt being dissolved in the second organic solvent; and mixing the cluster electrolyte precursor with the diaphragm matrix raw material, so that the first organic solvent in the diaphragm matrix raw material is volatilized to form a diaphragm matrix, so that the molecules of the second organic solvent in the cluster electrolyte precursor are combined with the lithium salt to form a cluster electrolyte, and the second organic solvent that has not formed the cluster electrolyte is volatilized to form the electrolyte diaphragm. It should be noted that those skilled in the art should understand that the molecules of the first organic solvent may not be completely volatilized due to the intermolecular forces generated by the molecules of the second organic solvent, etc., but the partial non-volatilization of the first organic solvent does not affect the formation of the diaphragm matrix and the cluster electrolyte.
[0044] The cluster electrolyte precursor is mixed with the diaphragm matrix raw material to prepare the electrolyte diaphragm, that is, during the preparation of the diaphragm matrix, the cluster electrolyte is formed in situ inside the diaphragm matrix, so that the cluster electrolyte can be evenly dispersed in the diaphragm matrix, thereby improving the ionic conductivity of the electrolyte diaphragm.
[0045] The cluster electrolyte includes complex molecules generated by complex reaction between cations of the lithium salt and molecules of the second organic solvent, and anions of the lithium salt located in the solvation sheath of the cations, and the cluster electrolyte is uniformly dispersed in the separator matrix.
[0046] In some embodiments, the high molecular polymer includes at least one of polyacrylonitrile, polyurethane, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyacrylate and polylactic acid.
[0047] In some embodiments, the first organic solvent includes at least one of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, acetone, tetrahydrofuran, acetonitrile, ethyl acetate, toluene and xylene.
[0048] In some embodiments, the lithium salt includes at least one of lithium trifluoromethylsulfonate, lithium bistrifluoromethylsulfonyl imide, lithium bisfluorosulfonyl imide, lithium di(polyfluoroalkylsulfonyl)imide, lithium di(polyfluoroalkoxysulfonyl)imide, tri(trifluoromethylsulfonyl)methyl lithium, lithium bisoxalatoborate, and lithium difluorooxalatoborate.
[0049] The second organic solvent includes at least one of a carbonate solvent, a fluorocarbon solvent, an ether solvent, a fluoroether solvent, a carboxylate solvent, a sulfite solvent, a phosphate solvent, and a sulfone solvent.
[0050] In some embodiments, the carbonate solvent includes at least one of ethylene carbonate, 1,2-dimethylethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, dibutyl carbonate and derivatives thereof.
[0051] In some embodiments, the fluorocarbonate solvent includes at least one of fluoroethylene carbonate, bisfluoroethylene carbonate, trifluoromethylethylene carbonate, methyl trifluoroethyl carbonate, fluorodimethyl carbonate and derivatives thereof.
[0052] In some embodiments, the ether solvent includes at least one of tetrahydrofuran, dioxolane, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol dibutyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether and derivatives thereof.
[0053] In some embodiments, the fluoroether solvent is a linear fluoroether with the structural formula: R 1 -OR 2 , where R 1 and R 2 It may be methyl, ethyl, propyl, isopropyl, butyl, sec-butyl, isobutyl, tert-butyl, pentyl, isopentyl, etc., or a group in which some or all of the hydrogen atoms are substituted with fluorine.
[0054] In some embodiments, the fluoroether solvent includes at least one of 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, 1,1,2,3,3,3-hexafluoropropyl-2,2,2-trifluoroethyl ether, 1,1,1,3,3,3-hexafluoropropyl-methyl ether, 1,1,1,2,3,3-hexafluoropropyl-2,2,3,3-tetrafluoropropyl ether and 1H,1H,5H-octafluoropentyl-1,1,2,2-tetrafluoroethyl ether.
[0055] In some embodiments, the carboxylate solvent includes at least one of methyl formate, methyl acetate, and ethyl acetate.
[0056] In some embodiments, the sulfite solvent includes at least one of dimethyl sulfite and diethyl sulfite.
[0057] In some embodiments, the phosphate ester solvent includes at least one of trimethyl phosphate, triethyl phosphate, tributyl phosphate, trioctyl phosphate, triphenyl phosphate, ethylene ethyl phosphate, and tris(2,2,2-trifluoroethyl) phosphate.
[0058] In some embodiments, the sulfone solvent includes at least one of dimethyl sulfoxide and sulfolane.
[0059] In some embodiments, the cluster electrolyte precursor further includes at least one of a performance optimizer and a flame retardant.
[0060] In some embodiments, the performance optimizer includes at least one of vinylene carbonate, vinylethylene carbonate, ethylene sulfate, ethylene sulfite, propylene sulfate, propylene sulfite, 4-methylethylene sulfate, 4-methylethylene sulfite, 1,4-butane sultone, 1,3-propane sultone, cyclohexylbenzene, tris(trimethylsilane)phosphate, tris(trimethylsilane)phosphite, tris(trimethylsilane)borate, succinonitrile, adiponitrile, pentafluoropropionic anhydride, fluoroethylene carbonate, lithium difluorooxalatoborate, lithium bistrifluoromethanesulfonyl imide, lithium bisfluorosulfonyl imide, lithium tetrafluoroborate, lithium bisoxalatoborate, lithium difluorophosphate, and lithium nitrate.
[0061] In some embodiments, the flame retardant includes at least one of tris(2,2,2-trifluoroethyl)phosphite, tris(4-fluorophenyl)phosphine, tris(2,2,3,3,3-pentafluoropropyl)phosphate, triphenyl phosphite, trimethyl phosphite, triethyl phosphite, tributyl phosphite, dimethyl methylphosphonate, diethyl ethylphosphonate, ethoxypentafluorocyclotriphosphazene, phenoxypentafluorocyclotriphosphazene, hexamethoxycyclotriphosphazene and ionic liquid.
[0062] In some embodiments, the cluster electrolyte precursor is mixed with the separator matrix raw material, the first organic solvent in the separator matrix raw material is volatilized to form a separator matrix, the molecules of the second organic solvent in the cluster electrolyte precursor are combined with the lithium salt to form a cluster electrolyte, and the second organic solvent that has not formed the cluster electrolyte is volatilized, and the method for forming the electrolyte separator includes:
[0063] Mixing the cluster electrolyte precursor with the separator matrix raw material to obtain a mixed solution; and
[0064] The mixed liquid is applied to the surface of the film-forming substrate, and the mixed liquid applied to the surface of the film-forming substrate is heated and / or negative pressure is applied to make the first organic solvent in the diaphragm matrix raw material evaporate to form a diaphragm matrix, make the molecules of the second organic solvent in the cluster electrolyte precursor combine with the lithium salt to form a cluster electrolyte, and make the second organic solvent that has not formed the cluster electrolyte evaporate to form the electrolyte diaphragm.
[0065] In some embodiments, the heating temperature is 30-120°C, for example, 30°C, 50°C, 70°C, 100°C or 120°C; and the heating time is 2-100h, for example, 2h, 10h, 50h, 80h or 100h.
[0066] In some embodiments, the negative pressure is applied by placing the film-forming substrate in a vacuum environment, such as a vacuum oven.
[0067] In some embodiments, the magnitude of the applied negative pressure is -0.02 MPa to -0.1 MPa, for example, -0.02 MPa, -0.05 MPa or -0.1 MPa.
[0068] In some embodiments, the cluster electrolyte precursor is mixed with the diaphragm matrix raw material, the first organic solvent in the diaphragm matrix raw material is volatilized to form a diaphragm matrix, the molecules of the second organic solvent in the cluster electrolyte precursor are combined with the lithium salt to form a cluster electrolyte, and the second organic solvent that has not formed the cluster electrolyte is volatilized. The method for forming the electrolyte diaphragm includes: mixing the cluster electrolyte precursor with the diaphragm matrix raw material to obtain a mixed liquid; and using the mixed liquid for electrospinning, the first organic solvent in the diaphragm matrix raw material is volatilized to form a diaphragm matrix, the molecules of the second organic solvent in the cluster electrolyte precursor are combined with the lithium salt to form a cluster electrolyte, and the second organic solvent that has not formed the cluster electrolyte is volatilized to form the electrolyte diaphragm.
[0069] In the third aspect, in addition to the preparation method of the electrolyte membrane described in the second aspect of the present application, the present application also provides another preparation method of the electrolyte membrane, including: providing a membrane substrate; providing a cluster electrolyte precursor, the cluster electrolyte precursor including a lithium salt and an organic solvent, the lithium salt being dissolved in the organic solvent; immersing the membrane substrate in the cluster electrolyte precursor or spraying the cluster electrolyte precursor onto the membrane substrate so that the cluster electrolyte precursor fills the interior and surface of the membrane substrate; and heating the membrane substrate and / or applying negative pressure so that the molecules of the organic solvent in the cluster electrolyte precursor combine with the lithium salt to form a cluster electrolyte, and volatilize the organic solvent that has not formed the cluster electrolyte, so as to obtain the electrolyte membrane.
[0070] The cluster electrolyte includes complex molecules generated by complex reaction between cations of the lithium salt and molecules of the organic solvent, and anions of the lithium salt located in the solvation sheath of the cations, and the cluster electrolyte is uniformly dispersed in the separator matrix.
[0071] The membrane matrix is a commonly used membrane in the prior art, and is a polymer membrane with a porous structure inside. In some embodiments, the material of the membrane matrix includes at least one of polyolefin, polyimide and cellulose.
[0072] In some embodiments, the membrane substrate is a single-layer or multi-layer porous polyolefin film, a porous polyimide film or a porous cellulose film.
[0073] In some embodiments, the separator substrate is a porous polyolefin film, a porous polyimide film or a porous cellulose film with a single-sided or double-sided coating.
[0074] The organic solvent includes at least one of a carbonate solvent, a fluorocarbon solvent, an ether solvent, a fluoroether solvent, a carboxylate solvent, a sulfite solvent, a phosphate solvent and a sulfone solvent.
[0075] In some embodiments, the lithium salt includes at least one of lithium trifluoromethylsulfonate, lithium bistrifluoromethylsulfonyl imide, lithium bisfluorosulfonyl imide, lithium di(polyfluoroalkylsulfonyl)imide, lithium di(polyfluoroalkoxysulfonyl)imide, tri(trifluoromethylsulfonyl)methyl lithium, lithium bisoxalatoborate, and lithium difluorooxalatoborate.
[0076] In some embodiments, the carbonate solvent includes at least one of ethylene carbonate, 1,2-dimethylethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, dibutyl carbonate and derivatives thereof.
[0077] In some embodiments, the fluorocarbonate solvent includes at least one of fluoroethylene carbonate, bisfluoroethylene carbonate, trifluoromethylethylene carbonate, methyl trifluoroethyl carbonate, fluorodimethyl carbonate and derivatives thereof.
[0078] In some embodiments, the ether solvent includes at least one of tetrahydrofuran, dioxolane, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, ethylene glycol dibutyl ether, diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, tetraethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether and derivatives thereof.
[0079] In some embodiments, the fluoroether solvent is a linear fluoroether with the structural formula: R 1 -OR 2 , where R 1 and R 2 It may be methyl, ethyl, propyl, isopropyl, butyl, sec-butyl, isobutyl, tert-butyl, pentyl, isopentyl, etc., or a group in which some or all of the hydrogen atoms are substituted with fluorine.
[0080] In some embodiments, the fluoroether solvent includes at least one of 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, 1,1,2,2-tetrafluoroethyl-2,2,3,3-tetrafluoropropyl ether, 1,1,2,3,3,3-hexafluoropropyl-2,2,2-trifluoroethyl ether, 1,1,1,3,3,3-hexafluoropropyl-methyl ether, 1,1,1,2,3,3-hexafluoropropyl-2,2,3,3-tetrafluoropropyl ether and 1H,1H,5H-octafluoropentyl-1,1,2,2-tetrafluoroethyl ether.
[0081] In some embodiments, the carboxylate solvent includes at least one of methyl formate, methyl acetate, and ethyl acetate.
[0082] In some embodiments, the sulfite solvent includes at least one of dimethyl sulfite and diethyl sulfite.
[0083] In some embodiments, the phosphate ester solvent includes at least one of trimethyl phosphate, triethyl phosphate, tributyl phosphate, trioctyl phosphate, triphenyl phosphate, ethylene ethyl phosphate, and tris(2,2,2-trifluoroethyl) phosphate.
[0084] In some embodiments, the sulfone solvent includes at least one of dimethyl sulfoxide and sulfolane.
[0085] In some embodiments, the cluster electrolyte precursor further includes at least one of a performance optimizer and a flame retardant.
[0086] In some embodiments, the performance optimizer includes at least one of vinylene carbonate, vinylethylene carbonate, ethylene sulfate, ethylene sulfite, propylene sulfate, propylene sulfite, 4-methylethylene sulfate, 4-methylethylene sulfite, 1,4-butane sultone, 1,3-propane sultone, cyclohexylbenzene, tris(trimethylsilane)phosphate, tris(trimethylsilane)phosphite, tris(trimethylsilane)borate, succinonitrile, adiponitrile, pentafluoropropionic anhydride, fluoroethylene carbonate, lithium difluorooxalatoborate, lithium bistrifluoromethanesulfonyl imide, lithium bisfluorosulfonyl imide, lithium tetrafluoroborate, lithium bisoxalatoborate, lithium difluorophosphate, and lithium nitrate.
[0087] In some embodiments, the flame retardant includes at least one of tris(2,2,2-trifluoroethyl)phosphite, tris(4-fluorophenyl)phosphine, tris(2,2,3,3,3-pentafluoropropyl)phosphate, triphenyl phosphite, trimethyl phosphite, triethyl phosphite, tributyl phosphite, dimethyl methylphosphonate, diethyl ethylphosphonate, ethoxypentafluorocyclotriphosphazene, phenoxypentafluorocyclotriphosphazene, hexamethoxycyclotriphosphazene and ionic liquid.
[0088] In some embodiments, the heating temperature is 30-120°C, for example, 30°C, 50°C, 70°C, 100°C or 120°C; and the heating time is 2-100h, for example, 2h, 10h, 50h, 80h or 100h.
[0089] In some embodiments, the negative pressure is applied by placing the membrane substrate in a vacuum environment, such as a vacuum oven.
[0090] In some embodiments, the magnitude of the applied negative pressure is -0.02 MPa, ~-0.1 MPa, for example, -0.02 MPa, -0.05 MPa or -0.1 MPa.
[0091] The specific implementation methods of the present application are further described below in combination with examples and comparative examples, but the present application is not limited to the following examples. The following examples are all conventional experimental methods unless otherwise specified; the reagents and materials used can be obtained from commercial channels unless otherwise specified.
[0092] Example 1
[0093] Take 5.8g of lithium bis(trifluoromethylsulfonyl)imide and add it to a mixed organic solvent of 13.5g of ethylene carbonate and 11.6g of dimethyl carbonate, stir it thoroughly to completely dissolve the lithium bis(trifluoromethylsulfonyl)imide, and continue stirring for 2h to form a cluster electrolyte precursor. Then immerse a polypropylene film with a porosity of 40% to 50% in the precursor solution for 10s, take it out and place it in an electric hot air drying oven at 100℃ to heat and dry it for 3h to obtain an electrolyte separator.
[0094] Example 2
[0095] Take 1.9g of lithium bis(fluorosulfonyl)imide and 2.9g of lithium bis(trifluoromethyl)sulfonyl)imide and add them to a mixed solvent consisting of 10.8g of dimethyl carbonate, 9.6g of ethyl methyl carbonate and 0.4g of vinylene carbonate, stir them thoroughly to completely dissolve the lithium bis(fluorosulfonyl)imide and lithium bis(trifluoromethyl)sulfonyl)imide, continue stirring for 2h to form a cluster electrolyte precursor. Add 20.6g of polyvinylidene fluoride solution (7%, N-methylpyrrolidone as solvent) to the cluster electrolyte precursor, stir them thoroughly to mix the two evenly to obtain a mixed solution. Use a film applicator to evenly coat the mixed solution on a glass plate, place the glass plate in a vacuum oven at 80°C, and dry it for 6h to obtain an electrolyte separator.
[0096] Example 3
[0097] The preparation method of the electrolyte membrane in Example 3 is roughly the same as the preparation method in Example 2, except that 3.1g of lithium bis(trifluoromethylsulfonyl imide) is added to 12.2g of diethyl carbonate, and the lithium bis(trifluoromethylsulfonyl imide) is fully stirred to completely dissolve, and stirring is continued for 2h to form a cluster electrolyte precursor. 19.6g of polyvinylidene fluoride-hexafluoropropylene solution (7%, N-methylpyrrolidone as solvent) is added to the cluster electrolyte precursor, and the mixture is fully stirred to mix the two to obtain a mixed solution. The mixed solution is evenly coated on a glass plate using a film applicator, and the glass plate is placed in a vacuum oven at 80°C for 6h to obtain an electrolyte membrane.
[0098] Example 4
[0099] Take 3.2g of lithium trifluoromethanesulfonate and add it to a mixed solvent consisting of 7.2g of propylene carbonate, 6.4g of dimethyl carbonate, 3.0g of ethylene glycol dimethyl ether and 0.3g of ethoxy pentafluorocyclotriphosphazene, stir it thoroughly to dissolve the lithium trifluoromethanesulfonate completely, and continue stirring for 2h to form a cluster electrolyte precursor. Add 21.4g of polyacrylonitrile solution (20%, N,N dimethylformamide as solvent) to the cluster electrolyte precursor, stir it thoroughly to mix the two evenly to obtain a mixed solution. Turn on the electrospinning equipment, set the voltage of the equipment to 16kV, the needle tube push speed to 0.9mL / h, the needle diameter to 0.4mm, the receiving distance to 13cm, and use electrospinning technology to spin the mixed solution into an electrolyte membrane.
[0100] Example 5
[0101] The preparation method of the electrolyte membrane in Example 5 is roughly the same as the preparation method in Example 4, except that 2.1g of lithium trifluoromethanesulfonate is added to 15.8g of trimethyl phosphate, and the lithium trifluoromethanesulfonate is fully stirred to dissolve completely, and stirring is continued for 2h to form a cluster electrolyte precursor. 19.2g of polyurethane solution (15%, tetrahydrofuran is solvent) is added to the cluster electrolyte precursor, and fully stirred to mix the two to obtain a mixed solution. The electrostatic spinning device is turned on, the voltage of the device is set to 15kV, the needle tube push speed is 0.7mL / h, the needle diameter is 0.5mm, and the receiving distance is 15cm. The mixed solution is spun into an electrolyte membrane using electrostatic spinning technology.
[0102] The electrolyte membrane prepared in the above example was subjected to room temperature ionic conductivity test and electrochemical window test, and the test method was as follows:
[0103] Room temperature ionic conductivity test
[0104] A symmetrical cell of blocking electrode / electrolyte membrane / blocking electrode was prepared using a polished stainless steel sheet as a blocking electrode, and the impedance of the electrolyte membrane prepared in Examples 1 to 5 was tested by electrochemical impedance spectroscopy (EIS) at room temperature. The room temperature ionic conductivity of the electrolyte membrane was calculated according to the formula: σ=d / (R*S), where σ is the room temperature ionic conductivity, d is the thickness of the electrolyte membrane, R is the impedance of the electrolyte membrane, and S is the effective contact area between the blocking electrode and the electrolyte membrane.
[0105] Electrochemical Window Test
[0106] A plugging electrode / electrolyte membrane / metallic lithium test cell was prepared using aluminum foil as the plugging electrode and metallic lithium as the counter electrode. The electrochemical window of the electrolyte membranes prepared in Examples 1 to 5 was tested by linear sweep voltammetry (LSV) at room temperature. The test voltage range was 2.0 V to 6.0 V, and the scan rate was 5 mV / s.
[0107] The above test results are shown in Table 1:
[0108] Table 1 Room temperature ionic conductivity and electrochemical window of electrolyte membranes prepared in Examples 1 to 5
[0109]
[0110] It can be seen from Table 1 that the electrolyte membranes prepared using the embodiments of the present application (Examples 1 to 5) have good room temperature ionic conductivity and a wider electrochemical window (the electrochemical window of liquid and gel electrolytes is usually ≤4.5V). Therefore, the electrolyte membrane provided by the present application can be applied to battery systems with high-voltage positive electrode materials, which can enable lithium batteries to have higher energy density.
[0111] In addition, the electrolyte membrane provided in the present application does not contain liquid organic electrolyte, so its thermal stability is better than that of gel electrolyte membrane. The electrolyte membrane provided in the present application does not require the use of high-cost solid electrolytes such as oxide solid electrolytes, sulfide solid electrolytes or polymer solid electrolytes during the preparation process, so its production cost is lower than that of solid electrolyte membrane.
[0112] In addition, the production process of the electrolyte membrane provided in the present application is simple, has the potential for large-scale application, and has important application value for the development of high-energy-density and high-safety lithium batteries.
[0113] In summary, after reading the contents of this application, those skilled in the art will appreciate that the aforementioned application contents may be presented only in an exemplary manner and may not be restrictive. Although not explicitly stated herein, those skilled in the art will appreciate that this application is intended to encompass various reasonable changes, improvements and modifications to the embodiments. These changes, improvements and modifications are within the spirit and scope of the exemplary embodiments of this application.
[0114] It should be understood that the term “and / or” used in this embodiment includes any or all combinations of one or more of the associated listed items.
[0115] Similarly, it should be understood that the terms "comprise", "comprising", "including" or "comprising", when used in this application document, indicate the presence of the recorded features, integers, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or groups thereof.
[0116] It should also be understood that although the terms first, second, third, etc. can be used to describe various elements, these elements should not be limited by these terms. These terms are only used to distinguish an element from another element. Therefore, without departing from the teaching of the application, the first element in some embodiments can be called the second element in other embodiments.
Claims
1. An electrolyte membrane, characterized in that: The invention comprises a diaphragm matrix and a cluster electrolyte uniformly dispersed in the diaphragm matrix, wherein the cluster electrolyte comprises complex molecules generated by complex reaction between cations of a lithium salt and molecules of an organic solvent, and anions of the lithium salt located in the solvation sheath of the cations, and the organic solvent comprises at least one of carbonate solvents, fluorocarbonate solvents, ether solvents, fluoroether solvents, carboxylate solvents, sulfite solvents, phosphate solvents and sulfone solvents.
2. The electrolyte membrane according to claim 1, characterized in that The lithium salt includes at least one of lithium trifluoromethylsulfonate, lithium bistrifluoromethylsulfonyl imide, lithium bisfluorosulfonyl imide, lithium di(polyfluoroalkylsulfonyl)imide, lithium di(polyfluoroalkoxysulfonyl)imide, tri(trifluoromethylsulfonyl)methyl lithium, lithium bisoxalatoborate and lithium difluorooxalatoborate.
3. The electrolyte membrane according to claim 1, characterized in that The material of the membrane substrate includes at least one of polyolefin, polyimide, cellulose, polyacrylonitrile, polyurethane, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyacrylate and polylactic acid.
4. The electrolyte membrane according to claim 1, characterized in that Also included are performance optimizers and / or flame retardants; The performance optimizer includes at least one of vinylene carbonate, vinylethylene carbonate, ethylene sulfate, ethylene sulfite, propylene sulfate, propylene sulfite, 4-methylethylene sulfate, 4-methylethylene sulfite, 1,4-butane sultone, 1,3-propane sultone, cyclohexylbenzene, tris(trimethylsilane) phosphate, tris(trimethylsilane) phosphite, tris(trimethylsilane) borate, succinonitrile, adiponitrile, pentafluoropropionic anhydride, fluoroethylene carbonate, lithium difluorooxalatoborate, lithium bistrifluoromethanesulfonyl imide, lithium bisfluorosulfonyl imide, lithium tetrafluoroborate, lithium bisoxalatoborate, lithium difluorophosphate and lithium nitrate; The flame retardant includes at least one of tris(2,2,2-trifluoroethyl)phosphite, tris(4-fluorophenyl)phosphine, tris(2,2,3,3,3-pentafluoropropyl)phosphate, triphenyl phosphite, trimethyl phosphite, triethyl phosphite, tributyl phosphite, dimethyl methylphosphonate, diethyl ethylphosphonate, ethoxy pentafluorocyclotriphosphazene, phenoxy pentafluorocyclotriphosphazene, hexamethoxycyclotriphosphazene and ionic liquid.
5. A method for preparing an electrolyte membrane, characterized in that: include: Providing a membrane matrix raw material, the membrane matrix raw material comprising a high molecular polymer and a first organic solvent, the high molecular polymer being dissolved in the first organic solvent; Providing a cluster electrolyte precursor, wherein the cluster electrolyte precursor comprises a lithium salt and a second organic solvent, wherein the lithium salt is dissolved in the second organic solvent; as well as The cluster electrolyte precursor is mixed with the separator matrix raw material, the first organic solvent in the separator matrix raw material is volatilized to form a separator matrix, the molecules of the second organic solvent in the cluster electrolyte precursor are combined with the lithium salt to form a cluster electrolyte, and the second organic solvent that has not formed the cluster electrolyte is volatilized to form the electrolyte separator; The cluster electrolyte includes complex molecules generated by complex reaction between cations of the lithium salt and molecules of the second organic solvent, and anions of the lithium salt located in the solvation sheath of the cations, and the cluster electrolyte is uniformly dispersed in the separator matrix; The second organic solvent includes at least one of a carbonate solvent, a fluorocarbon solvent, an ether solvent, a fluoroether solvent, a carboxylate solvent, a sulfite solvent, a phosphate solvent, and a sulfone solvent.
6. The method for preparing an electrolyte membrane according to claim 5, characterized in that: The lithium salt includes at least one of lithium trifluoromethylsulfonate, lithium bistrifluoromethylsulfonyl imide, lithium bisfluorosulfonyl imide, lithium di(polyfluoroalkylsulfonyl)imide, lithium di(polyfluoroalkoxysulfonyl)imide, tri(trifluoromethylsulfonyl)methyl lithium, lithium bisoxalatoborate and lithium difluorooxalatoborate.
7. The method for preparing an electrolyte membrane according to claim 5, characterized in that: The high molecular polymer includes at least one of polyacrylonitrile, polyurethane, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyacrylate and polylactic acid; and / or The first organic solvent includes at least one of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, acetone, tetrahydrofuran, acetonitrile, ethyl acetate, toluene and xylene.
8. The method for preparing an electrolyte membrane according to claim 5, characterized in that: The cluster electrolyte precursor further includes at least one of a performance optimizer and a flame retardant; The performance optimizer includes at least one of vinylene carbonate, vinylethylene carbonate, ethylene sulfate, ethylene sulfite, propylene sulfate, propylene sulfite, 4-methylethylene sulfate, 4-methylethylene sulfite, 1,4-butane sultone, 1,3-propane sultone, cyclohexylbenzene, tris(trimethylsilane)phosphate, tris(trimethylsilane)phosphite, tris(trimethylsilane)borate, succinonitrile, adiponitrile, pentafluoropropionic anhydride, fluoroethylene carbonate, lithium difluorooxalatoborate, lithium bistrifluoromethanesulfonyl imide, lithium bisfluorosulfonyl imide, lithium tetrafluoroborate, lithium bisoxalatoborate, lithium difluorophosphate and lithium nitrate; and The flame retardant includes at least one of tris(2,2,2-trifluoroethyl)phosphite, tris(4-fluorophenyl)phosphine, tris(2,2,3,3,3-pentafluoropropyl)phosphate, triphenyl phosphite, trimethyl phosphite, triethyl phosphite, tributyl phosphite, dimethyl methylphosphonate, diethyl ethylphosphonate, ethoxy pentafluorocyclotriphosphazene, phenoxy pentafluorocyclotriphosphazene, hexamethoxycyclotriphosphazene and ionic liquid.
9. The method for preparing an electrolyte membrane according to claim 5, characterized in that: The method of forming the electrolyte membrane by mixing the cluster electrolyte precursor with the separator matrix raw material, volatilizing the first organic solvent in the separator matrix raw material to form a separator matrix, combining the molecules of the second organic solvent in the cluster electrolyte precursor with the lithium salt to form a cluster electrolyte, and volatilizing the second organic solvent that has not formed the cluster electrolyte, comprises: Mixing the cluster electrolyte precursor with the separator matrix raw material to obtain a mixed solution; and The mixed liquid is applied to the surface of the film-forming substrate, and the mixed liquid applied to the surface of the film-forming substrate is heated and / or negative pressure is applied to make the first organic solvent in the diaphragm matrix raw material evaporate to form a diaphragm matrix, make the molecules of the second organic solvent in the cluster electrolyte precursor combine with the lithium salt to form a cluster electrolyte, and make the second organic solvent that has not formed the cluster electrolyte evaporate to form the electrolyte diaphragm.
10. The method for preparing an electrolyte membrane according to claim 5, characterized in that: The method of forming the electrolyte membrane by mixing the cluster electrolyte precursor with the separator matrix raw material, volatilizing the first organic solvent in the separator matrix raw material to form a separator matrix, combining the molecules of the second organic solvent in the cluster electrolyte precursor with the lithium salt to form a cluster electrolyte, and volatilizing the second organic solvent that has not formed the cluster electrolyte, comprises: The cluster electrolyte precursor is mixed with the diaphragm matrix raw material to obtain a mixed solution; and The mixed solution is used for electrospinning, so that the first organic solvent in the membrane matrix raw material is volatilized to form a membrane matrix, the molecules of the second organic solvent in the cluster electrolyte precursor are combined with the lithium salt to form a cluster electrolyte, and the second organic solvent that has not formed the cluster electrolyte is volatilized to form the electrolyte membrane.