Stator coil main insulation structure for improving VPI permeability and manufacturing method thereof
By using a combination structure of a high-breathable, low-glue powder mica tape and an alkali-free glass fiber cloth in the stator coil, cross-space bandage and dry dot-like glue production, the problems of uneven filling of impregnated resin and long holding time are solved. , improves insulation performance and production efficiency, and ensures the safety and reliability of the motor unit.
Patent Information
- Application Number
- CN202411298141.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-11-19
AI Technical Summary
In the prior art, when the main insulation thickness of the stator coil increases, the VPI impregnated resin is filled unevenly, resulting in unqualified insulation performance, and long-term pressure holding will cause mica scales to move, resulting in low industrial frequency breakdown voltage and short electrical aging time. question.
The main insulating structure consisting of high breathable, low-glue powder mica tape of different thicknesses and alkali-free glass fiber cloth is made by dry dot glue, cross-dressing, shortening the VPI impregnation and holding pressure time, and at 150℃±5 The curing treatment was carried out for 10 hours at a temperature of °C.
It improves the fluidity and permeability of the impregnated resin, reduces insulation performance defects, shortens VPI pressure holding time, ensures long-term safe and reliable operation of the stator coil, and reduces production costs and energy consumption.
Smart Images

Figure CN118983973A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of stator coil insulation, and more particularly to a stator coil main insulation structure for improving VPI permeability and a manufacturing method thereof. Background Art
[0002] The stator coil is the core component of the motor. The permeability of the main insulation VPI determines the electrical and mechanical properties of the stator coil, and plays a vital role in the safe and reliable operation of the generator set. There are two main insulation systems for the stator coil main insulation. One is an insulation system in which the surface of the conductor is covered with a mica tape with less glue powder, and the epoxy resin is vacuum pressure impregnated and then hot-pressed and cured (referred to as the VPI insulation system with less glue, the same below); the other is an insulation system in which the surface of the conductor is covered with a mica tape with more glue powder, and the insulation system is directly hot-pressed and cured (referred to as the multi-glue insulation system, the same below).
[0003] At present, the conventional method for domestic and foreign motor manufacturers to produce VPI stator coil insulation for high-voltage motors is as follows: after the coil wire is cured and formed, different layers of low-glue mica tape are half-wrapped on the surface of the coil wire according to the rated voltage of the motor. After the coil is placed in a paint pot, the paint pot is evacuated, and the impregnation resin is input into the paint pot. A certain pressure is applied to the resin in the paint pot and maintained at this pressure for a period of time. Then the pressure in the paint pot is removed, the VPI resin is withdrawn, and the coil is taken out for hot pressing and curing.
[0004] The main factors affecting the VPI permeability of the stator coil main insulation are the thickness of the coil main insulation, the air permeability of the main insulation mica tape, the pressure holding time during the VPI process, and the viscosity of the impregnation resin. As the rated voltage level of the motor increases, the thickness of the coil main insulation will also increase. The thicker the coil main insulation, the longer the VPI pressure holding time required. When the stator coil main insulation is thicker, the impregnation resin is not completely immersed in the inner mica tape, and the resin filling between the mica tape layers is uneven, causing the coil main insulation to be hollow, with too many air gaps, and poor interlayer bonding, resulting in large coil dielectric loss increments and local discharge values, low power frequency breakdown voltage, short electrical aging time, and other insulation performance failures. Therefore, in order to make the inner main insulation mica layer penetrate, the penetration time is usually extended. However, too long an impregnation time will cause the mica flakes in the main insulation mica tape to move and move, resulting in low power frequency breakdown voltage, short electrical aging time, and other insulation performance failures in the coil main insulation. Summary of the invention
[0005] The present invention proposes a stator coil main insulation structure with improved VPI permeability and a manufacturing method thereof. The present invention can not only improve the fluidity of the impregnating resin between mica tape layers, but also shorten the VPI impregnation and pressure holding time, so that the resin filling between the mica tape layers is uniform, reduce the VPI defects of the stator coil main insulation, reduce the quality loss caused by unqualified coil insulation performance, and ensure the stable reliability of the long-term safe operation of the unit.
[0006] In order to achieve the above-mentioned object of the invention, the technical solution of the present invention is as follows:
[0007] On the one hand, the present invention discloses a stator coil main insulation structure for improving VPI permeability, wherein the main insulation structure is composed of high-permeability, low-rubber powder mica tape and alkali-free glass fiber cloth of different thicknesses; wherein the high-permeability, low-rubber powder mica tape includes two types, the first type of high-permeability, low-rubber powder mica tape has a thickness of 0.15 mm, a mica content greater than 80%, an epoxy curing agent content of 7% to 8%, and an air permeability of ≤500s / 100mL; the second type of high-permeability, low-rubber powder mica tape has a thickness of 0.11 mm, a mica content greater than 60%, an epoxy curing agent content of 7% to 8%, and an air permeability of ≤300s / 100mL; the alkali-free glass fiber cloth has a thickness of 0.06 mm to 0.10 mm, and an air permeability of ≤100s / 100mL.
[0008] Preferably, the stator coil main insulation structure comprises alkali-free glass fiber cloth, a first type of high-air permeability low-rubber powder mica tape, and a second type of high-air permeability low-rubber powder mica tape, which are half-folded on the surface of the coil copper conductor from the inside to the outside.
[0009] Preferably, the stator coil main insulation structure includes an alkali-free glass fiber cloth half-folded and wrapped on the surface of the coil copper conductor from the inside to the outside, and a first type of high-permeability, low-rubber powder mica tape and a second type of high-permeability, low-rubber powder mica tape wrapped cross-spaced.
[0010] In the present invention, two kinds of high-air-permeability and low-glue mica tapes are made by dry point-shaped gluing.
[0011] Based on the same inventive concept, the present invention also discloses a method for preparing a stator coil main insulation structure for improving VPI permeability. The preparation method is used to prepare the above-mentioned stator coil main insulation structure. The specific preparation method is as follows: Step S1. After the stator coil wire is hot-pressed, a layer of alkali-free glass fiber cloth is half-wrapped on the surface of the coil copper conductor, and the single-sided binding thickness of the alkali-free glass fiber cloth is d1;
[0012] Step S2. After the alkali-free glass fiber cloth is wrapped, the first type of high-air-permeability, low-glue mica tape is half-wrapped on the surface of the coil copper conductor, and the wrapping thickness is d2;
[0013] Step S3. After the stator coil is wrapped with the first high-permeability and low-rubber-powder mica tape, the second high-permeability and low-rubber-powder mica tape is wrapped on its surface, and the wrapping method is half-folded or flat, and the wrapping thickness is d3;
[0014] Step S4. Then, the first high-permeability and low-rubber-powder mica tape and the second high-permeability and low-rubber-powder mica tape are cross-wrapped at intervals until the total thickness d of the stator coil main insulation structure design is reached;
[0015] Step S5. After the stator coil main insulation wrapping is completed, VPI is performed on the stator coil. After the coil main insulation is pressurized in the mold, it is placed in a drying oven for heating and curing. The curing temperature is 150°C±5°C and the curing time is 10 hours. The mold is cooled to below 100°C and then taken out of the oven.
[0016] Preferably, the thickness of the first high-permeability, low-rubber-powder mica tape and the second high-permeability, low-rubber-powder mica tape for each wrapping are the same, and the relationship between the total thickness d of the stator coil main insulation and the thickness of each layer of main insulation is as follows:
[0017] d = d1 + k1 × d2 + (k1-1) × d3;
[0018] Among them, k1 represents the number of times the first type of high-air permeability and low-glue mica tape is wrapped.
[0019] Preferably, the limit values of the wrapping thickness d2 of the first high-air-permeability low-rubber-powder mica tape and the wrapping thickness d3 of the second high-air-permeability low-rubber-powder mica tape are as follows:
[0020]
[0021] The method for preparing a stator coil main insulation structure with improved VPI permeability according to claim 4 is characterized in that during the curing process, the curing temperature is 150°C ± 5°C and the curing time is 10 hours.
[0022] Beneficial effects of the present invention:
[0023] 1. The main insulation structure of the stator coil of the present invention is composed of high-permeability, low-glue mica tape and alkali-free glass fiber cloth with different insulation thicknesses, which not only shortens the VPI impregnation and pressure holding time, but also improves the fluidity and permeability of the impregnating resin between the mica tape layers, so that the resin filling between the mica tape layers is uniform, reduces the VPI defects of the stator coil main insulation, reduces the quality loss caused by unqualified coil insulation performance, and ensures the timely and quality delivery of the stator coil and the stable reliability of the long-term safe operation of the unit.
[0024] 2. The stator coil prepared by the method of the present invention has a smaller dielectric loss increment and partial discharge value, the main insulation permeability of the stator coil is better than that of the conventional structure, and the VPI pressure holding time of the stator coil is shortened by 20% to 30%, which effectively improves production efficiency, reduces energy consumption, and reduces production costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The foregoing and following detailed description of the present invention will become more apparent when read in conjunction with the following drawings, in which:
[0026] Figure 1 This is a schematic diagram of the main insulation structure of the stator coil in Example 1 of the present invention;
[0027] Figure 2 This is a schematic diagram of the main insulation structure of the stator coil in Embodiment 2 of the present invention;
[0028] In the figure:
[0029] 1. Copper conductor; 2. Alkali-free glass fiber cloth; 3. The first type of high air permeability and low-glue mica tape; 4. The second type of high air permeability and low-glue mica tape. DETAILED DESCRIPTION
[0030] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions for achieving the purpose of the present invention will be further described below through several specific embodiments. It should be noted that the technical solutions claimed for protection in the present invention include but are not limited to the following embodiments. Based on the embodiments in the present invention, all other embodiments obtained by those skilled in the art without creative work shall fall within the scope of protection of the present invention.
[0031] An embodiment of the present invention provides a stator coil main insulation structure for improving VPI permeability suitable for 18kV-35kV high-voltage motors and a manufacturing method thereof. The main insulation structure of the stator coil of the present invention is composed of highly air-permeable, low-glue mica tape and alkali-free glass fiber cloth of different insulation thicknesses, which can not only shorten the VPI impregnation and pressure holding time, but also improve the fluidity and permeability of the impregnating resin between mica tape layers, so that the resin filling between mica tape layers is uniform, reducing the VPI defects of the stator coil main insulation, thereby reducing the quality loss caused by unqualified insulation performance of the stator coil, ensuring the timely and quality delivery of the stator coil and the stable reliability of the long-term safe operation of the unit.
[0032] The present invention will be explained and illustrated in more detail below in conjunction with specific implementation methods.
[0033] Example 1
[0034] This embodiment uses the stator coil main insulation structure manufacturing method proposed in the present invention to manufacture the stator coil main insulation structure with a rated voltage of 26 kV and a main insulation single-side design thickness of 6.0 mm. First, a 0.10mm alkali-free glass fiber cloth is half-wrapped on the surface of the copper conductor of the coil, and the thickness of the single wrap is 0.2mm; then the first high-permeability and low-rubber powder mica tape is wrapped, a total of 6 half-wrapped layers, and the thickness of the single wrap is 1.8mm; then the second high-permeability and low-rubber powder mica tape is wrapped, the wrapping method is half-wrapped, the number of wrapping layers is one layer, and the thickness of the single wrap is 0.2mm; continue to wrap the first high-permeability and low-rubber powder mica tape, half-wrapped 6 layers, and the thickness of the single wrap is 1.8mm; then half-wrapped a layer of the second high-permeability and low-rubber powder mica tape, the thickness of the single wrap is 0.2mm; then the first high-permeability and low-rubber powder mica tape is wrapped, half-wrapped 6 layers, and the thickness of the single wrap is 1.8mm; after the wrapping is formed, the final main insulation wrapping has a total thickness of 6.0mm, and a total of three layers of impregnated resin flow channels are formed, such as Figure 1 shown.
[0035] Figure 1 The stator coil main insulation structure finally formed in this embodiment is composed of Figure 1 It can be seen that from the inside to the outside, they are alkali-free glass fiber cloth, the first type of high air permeability low rubber powder mica tape, the second type of high air permeability low rubber powder mica tape, the first type of high air permeability low rubber powder mica tape, the second type of high air permeability low rubber powder mica tape and the first type of high air permeability low rubber powder mica tape.
[0036] After the stator coil main insulation is wrapped and formed, the stator coil is subjected to VPI. After the coil main insulation is pressurized in the mold, it is placed in a drying oven for heating and curing. The curing temperature is 150℃±5℃ and the curing time is 10h. The mold is cooled to below 100℃ and then taken out of the oven. The stator coil VPI pressure holding time is 7h.
[0037] Example 2
[0038] This embodiment uses the manufacturing method of the stator coil main insulation structure proposed in the present invention to manufacture the main insulation structure of the stator coil with a rated voltage of 26kV and a main insulation single-sided design thickness of 6.0mm. First, half-wrap a layer of 0.10mm alkali-free glass fiber cloth on the surface of the copper conductor of the stator coil, and the thickness of the single-sided wrapping is 0.2mm; then wrap the first high-permeability, low-rubber powder mica tape, half-wrap 10 layers in total, and the thickness of the single-sided wrapping is 3.0mm; then wrap the second high-permeability, low-rubber powder mica tape, half-wrap 2 layers in total, and the thickness of the single-sided wrapping is 0.4mm; continue to wrap the first high-permeability, low-rubber powder mica tape, half-wrap 8 layers in total, and the thickness of the single-sided wrapping is 2.4mm; after wrapping and forming, two layers of resin-impregnated flow channels are formed, such as Figure 2 shown.
[0039] Figure 2 The stator coil main insulation structure finally formed in this embodiment is composed of Figure 2 It can be seen that from the inside to the outside, they are alkali-free glass fiber cloth, the first type of high air permeability low rubber powder mica tape, the second type of high air permeability low rubber powder mica tape and the first type of high air permeability low rubber powder mica tape.
[0040] In all the embodiments described in the present invention, the first high-permeability, low-glue mica tape used in the above-mentioned embodiments 1-2 has a thickness of 0.15 mm, a mica content greater than 80%, an epoxy curing agent content of 7% to 8%, and an air permeability of ≤500s / 100mL; the second high-permeability, low-glue mica tape has a thickness of 0.11 mm, a mica content greater than 60%, an epoxy curing agent content of 7% to 8%, and an air permeability of ≤300s / 100mL; and both of the above-mentioned mica tapes are formed by dry dot gluing.
[0041] Example 3
[0042] This embodiment uses a conventional stator coil main insulation structure manufacturing method to manufacture a stator coil main insulation structure with a rated voltage of 26 kV and a main insulation design thickness of 6.0 mm. The stator coil main insulation wrapping method is to continuously half-wrap 20 layers of 0.15 mm thick epoxy low-glue mica tape on the surface of the coil copper conductor, and then perform VPI on the coil.
[0043] Example 4
[0044] In this embodiment, VPI is performed on the stator coil main insulation structure prepared in the above embodiments 1 to 3 to obtain the stator coil main insulation structure and VPI pressure holding time shown in Table 1 below.
[0045] Table 1 Comparison of stator coil main insulation structure and VPI pressure holding time
[0046]
[0047] It can be seen from the VPI pressure holding test data in Table 1 that the stator coil main insulation structure prepared by the present invention can significantly shorten the impregnation pressure holding time and improve production efficiency compared with the stator coil main insulation structure prepared by the conventional method.
[0048] Example 5
[0049] In this embodiment, the stator coils prepared in the above-mentioned embodiments 1 to 3 are baked and cured, and then their insulation properties are tested. The test results are shown in Table 2. Among them, coils 1-1# to 1-6# are stator coils prepared by conventional methods in embodiment 3, and coils 2-1# to 2-6# are stator coils prepared in embodiment 1.
[0050] Table 2 Stator coil insulation performance test table
[0051]
[0052] From the test data of the starting value of dielectric loss, dielectric loss increment, partial discharge value under line voltage, instantaneous power frequency breakdown voltage value and 3 times aging time of the stator coil after VPI baking and curing in Table 2, it can be seen that the stator coil prepared by the stator coil main insulation structure manufacturing method proposed in the present invention has smaller dielectric loss increment and partial discharge value, and the permeability of the stator coil main insulation structure is better than that of the stator coil main insulation structure prepared by the conventional method.
[0053] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the scope of protection of the present invention.
[0054] In the description of the present invention, it is also necessary to explain that, unless otherwise clearly specified and limited, the terms "setting", "installation" and "connection" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be an indirect connection through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0055] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification or equivalent change made to the above embodiment based on the technical essence of the present invention shall fall within the protection scope of the present invention.
Claims
1. A stator coil main insulation structure for improving VPI permeability, characterized in that: The stator coil main insulation structure is composed of high-permeability, low-rubber powder mica tape and alkali-free glass fiber cloth of different thicknesses; wherein the high-permeability, low-rubber powder mica tape includes two types, the first type of high-permeability, low-rubber powder mica tape has a thickness of 0.15mm, a mica content greater than 80%, an epoxy curing agent content of 7% to 8%, and an air permeability of ≤500s / 100mL; the second type of high-permeability, low-rubber powder mica tape has a thickness of 0.11mm, a mica content greater than 60%, an epoxy curing agent content of 7% to 8%, and an air permeability of ≤300s / 100mL; the alkali-free glass fiber cloth has a thickness of 0.06mm to 0.10mm, and an air permeability of ≤100s / 100mL.
2. A stator coil main insulation structure for improving VPI permeability according to claim 1, characterized in that: The stator coil main insulation structure comprises alkali-free glass fiber cloth, a first type of high-air permeability low-rubber powder mica tape and a second type of high-air permeability low-rubber powder mica tape which are half-folded and wrapped on the surface of the coil copper conductor from the inside to the outside.
3. A stator coil main insulation structure for improving VPI permeability according to claim 1, characterized in that: The stator coil main insulation structure includes an alkali-free glass fiber cloth half-folded and wrapped on the surface of the coil copper conductor from the inside to the outside, and a first high-permeability low-rubber powder mica tape and a second high-permeability low-rubber powder mica tape wrapped in a cross-interval.
4. A method for manufacturing a stator coil main insulation structure with improved VPI permeability, the method being used to prepare the stator coil main insulation structure according to any one of claims 1 to 3, characterized in that: The following steps are involved: Step S1. After the stator coil conductor is hot-pressed, a layer of alkali-free glass fiber cloth is half-wrapped on the surface of the coil copper conductor, and the single-sided wrapping thickness of the alkali-free glass fiber cloth is d1; Step S2. After the alkali-free glass fiber cloth is wrapped, the first type of high-air-permeability, low-glue mica tape is half-wrapped on the surface of the coil copper conductor, and the wrapping thickness is d2; Step S3. After the stator coil is wrapped with the first high-permeability and low-rubber-powder mica tape, the second high-permeability and low-rubber-powder mica tape is wrapped on its surface, and the wrapping method is half-folded or flat, and the wrapping thickness is d3; Step S4. Then, the first high-permeability and low-rubber-powder mica tape and the second high-permeability and low-rubber-powder mica tape are cross-wrapped at intervals until the total thickness d of the stator coil main insulation structure design is reached; Step S5. After the stator coil main insulation wrapping is completed, VPI is performed on the stator coil. After the coil main insulation is pressurized in the mold, it is placed in a drying oven for heating and curing. The curing temperature is 150°C±5°C and the curing time is 10 hours. The mold is cooled to below 100°C and then taken out of the oven.
5. The method for preparing a stator coil main insulation structure for improving VPI permeability according to claim 4, characterized in that: The thickness of the first type of high-permeability, low-rubber-powder mica tape and the thickness of the second type of high-permeability, low-rubber-powder mica tape are the same for each wrapping. The relationship between the total thickness d of the stator coil main insulation and the thickness of each layer of main insulation is as follows: d = d1 + k1 × d2 + (k1-1) × d3; Among them, k1 represents the number of times the first type of high-air permeability and low-glue mica tape is wrapped.
6. A method for manufacturing a stator coil main insulation structure for improving VPI permeability according to claim 4, characterized in that: The limits of the wrapping thickness d2 of the first type of high-air-permeability and low-glue-powder mica tape and the wrapping thickness d3 of the second type of high-air-permeability and low-glue-powder mica tape are as follows:
7. A method for manufacturing a stator coil main insulation structure for improving VPI permeability according to claim 4, characterized in that: During solidification, the curing temperature is 150℃±5℃ and the curing time is 10h.