Thermoelectric leg and preparation method thereof

By using foam metal material as a metal layer in the thermoelectric legs, embedded thermoelectric material powder is to enhance the shear strength, and connecting thermoelectric devices through non-brazing methods, the shear strength of metal layers and thermoelectric materials in the prior art is solved. The problems of low and low yields achieve higher connection strength and wider process selection.

CN118984640APending Publication Date: 2024-11-19WUHAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411051942.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

In the existing thermoelectric leg preparation process, the shear strength of the metal layer and the thermoelectric material is low, and the yield of the micro-size thermoelectric column is low, the process flow is complex and the cost is high.

Method used

The foam metal material is used as the metal layer, and the thermoelectric material powder is embedded in the foam metal holes through the sintering process to enhance mechanical occlusion, improve shear strength, and connect thermoelectric devices through non-brazing methods to broaden the range of process selection.

Benefits of technology

The connection strength between the metal layer and thermoelectric material is improved, the connection strength of the brazed joint is improved, the thickness unevenness of the metal layer is reduced, the yield of micro-size thermoelectric columns is improved, and the preparation process selection of thermoelectric devices is broadened.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118984640A_ABST
    Figure CN118984640A_ABST
Patent Text Reader

Abstract

The invention provides a thermoelectric leg and a preparation method thereof, and belongs to the field of thermoelectric elements. The two metal layers are attached to the upper end face and the lower end face of the thermoelectric column. The thermoelectric material adopts one or more of Bi-Te-based alloy, CoSb3-based skutterudite, Pb-Te-based alloy, Sn-Te alloy, Cu-Se alloy, Half-Heusler alloy and a Zintl phase compound, and the metal layer is made of a foam metal material; compared with a physical vapor deposition method, the method has the advantages that the technological process is reduced, the selection range of technological parameters of foam metal is larger than that of powder, the thickness of a metal layer sintered by alloy powder is more uniform, the thickness of the metal layer is greatly reduced, the machining yield of the micro-size thermoelectric column is increased, and the production cost is reduced. And the selection range of the preparation process of the thermoelectric device is widened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of thermoelectric elements, and in particular to a thermoelectric leg and a preparation method thereof. Background Art

[0002] Thermoelectric devices can realize the direct conversion between heat and electricity. The π-type thermoelectric device is based on the thermoelectric leg. In the production process of thermoelectric legs, physical vapor deposition is usually used to grow one or more metal layers on the upper and lower ends of the thermoelectric leg blank. The metal layer plays the role of metallization layer, barrier layer or transition layer to improve the electrical and mechanical properties of the thermoelectric leg and the metal electrode. At present, there are also many reports on the method of using alloy powder, foil, sheet and thermoelectric material to sinter together to achieve the simultaneous preparation of metal layer and thermoelectric leg.

[0003] Chinese patent CN102648538A discloses the use of porous metal materials as contact connections in thermoelectric modules, wherein the thermoelectric module is composed of p and n conductive thermoelectric material columns alternately connected to each other through conductive contacts, so that the conductive contacts located on the cold side and / or hot side of the thermoelectric module are made of porous metal materials and formed between the thermoelectric material columns or embedded in the thermoelectric material columns.

[0004] However, the prior art still has the following disadvantages:

[0005] (1) The metal layer prepared by the traditional physical vapor deposition method has the disadvantages of multiple preparation processes and high production costs;

[0006] (2) The current method of preparing thermoelectric legs by sintering alloy powders and thermoelectric materials together has the following process disadvantages: the thickness of the metal layer is difficult to control uniformly; in order to make the alloy powder sinter densely, the sintering pressure and temperature are relatively high, which limits the range of choice of process parameters;

[0007] (3) The metal layers prepared by the above two methods (1) and (2) as well as the metal layers prepared using metal foils and sheets have the disadvantages of low shear strength between the metal layer and the thermoelectric material and low yield of micro-sized thermoelectric columns.

[0008] In summary, the existing technology still has a lot of room for improvement. Summary of the invention

[0009] In view of this, the present invention proposes a thermoelectric leg and a preparation method thereof, which are used to solve the problems of low shear strength between the metal layer and the thermoelectric material and low yield of micro-sized thermoelectric columns in the current preparation process.

[0010] The technical solution of the present invention is implemented as follows: the present invention provides a thermoelectric leg, including a thermoelectric column, which is made of thermoelectric material; two metal layers are attached to the upper and lower end faces of the thermoelectric column; wherein the thermoelectric material adopts one or more of Bi-Te based alloy, CoSb3 based skutterudite, Pb-Te based alloy, Sn-Te alloy, Cu-Se alloy, Half-Heusler alloy, Zintl phase compound, and the metal layer is made of foam metal material. Thermoelectric material is a kind of material that can directly convert thermal energy into electrical energy, or convert electrical energy into thermal energy. This bidirectional energy conversion characteristic makes thermoelectric materials have important application value in the fields of energy conversion and refrigeration. The working principle of thermoelectric materials is based on the thermoelectric effect, which mainly includes three effects: first, the Seebeck effect. When there is a temperature difference between the two ends of the thermoelectric material, a voltage difference will be generated between the two ends, which can convert thermal energy into electrical energy; second, the Peltier effect. When current passes through the contact point of two different conductors or semiconductors, it absorbs or releases heat at the contact point, thereby achieving cooling or heating; third, the Thomson effect. When current passes through a single conductor with a temperature gradient, the conductor absorbs or releases heat. The principle of the present invention is that the thermoelectric material powder will be embedded in the pores of the foam material during the sintering process, and after sintering, it will form a mechanical bite with the foam metal, thereby enhancing the shear strength between the thermoelectric material and the metal layer. Figure 4 The SEM image of the interface between the foam metal and the thermoelectric material powder after sintering shown in (b) shows the effect of mechanical interlocking between the foam metal and the thermoelectric material. The mechanical interlocking between the foam metal and the thermoelectric material simultaneously strengthens the surface of the thermoelectric material, enhances the surface strength of the thermoelectric material, and can have a higher yield in the process of preparing micro-sized thermoelectric columns. After sintering, the foam metal will have tiny holes on its surface. These holes enhance the capillary action of the solder, improve the wettability of the solder on the surface of the metal layer, and thus enhance the connection strength of the brazed joint. In addition, the thermoelectric column prepared by the present invention can also be connected to the metal electrode of the thermoelectric device by non-brazing methods such as resistance welding, which broadens the range of choices for the preparation process of the thermoelectric device.

[0011] On the basis of the above technical solutions, preferably, the foam metal adopts one or more of foam Ni, foam Fe and its alloys, foam Cu, foam Al, and foam Ti. Foam metal is a special metal material, which is filled with a large number of bubbles or holes inside, giving it a foam-like structure. The porosity of foam metal is usually very high, reaching 75% to 95%, which makes it lighter than traditional metals while retaining certain mechanical strength and thermal conductivity. Foam metal can be divided into open-cell foam and closed-cell foam. The holes inside the open-cell foam metal are interconnected, similar to a sponge, so that the open-cell foam metal has good air permeability and filtering properties, and is suitable for applications such as filters and heat dissipation materials; the holes inside the closed-cell foam metal are closed and not interconnected, so that the closed-cell foam metal has higher sound insulation and heat insulation properties, and is suitable for applications such as lightweight structural materials and energy-absorbing materials. The present invention adopts open-cell foam metal. As Figure 5 The figure shows a SEM image of a metal layer formed by sintered foamed metal, which demonstrates that the metal layer formed by the preparation method of the present invention has a higher density.

[0012] On the basis of the above technical solution, preferably, the thickness of the metal layer before sintering is ≤5 mm, and the porosity is 90% to 95%.

[0013] More preferably, the thickness of the metal layer after sintering is less than 0.2 mm.

[0014] On the basis of the above technical solution, preferably, it also includes two substrates, which are spaced apart from each other and at least one thermoelectric column is arranged between the two substrates; a solder layer is arranged between the surface of the substrate and the end face of the metal layer where the thermoelectric column is arranged, and is used to connect the substrate and the metal layer and make the two contact with each other in a thermally conductive manner.

[0015] On the other hand, the present invention also provides a method for preparing a thermoelectric leg, comprising the following steps: step one, weighing the required mass of thermoelectric material powder according to the product requirements of the thermoelectric leg, cutting the foam metal raw material into a shape consistent with the inner diameter of the graphite mold, and sequentially loading the foam metal raw material, the thermoelectric material powder and the foam metal raw material into the graphite mold; step two, placing the graphite mold filled with the raw materials into a spark plasma sintering system for sintering, applying axial pressure to the raw materials in the graphite mold during the sintering process, and obtaining a blank after sintering; step three, roughly grinding the upper and lower surfaces of the blank, then using a wire cutting machine to cut the blank into thermoelectric legs of the required size, and fine grinding the surface of the thermoelectric legs.

[0016] On the basis of the above technical solution, preferably, the axial pressure applied to the raw material in step 2 is 10 MPa to 40 MPa.

[0017] On the basis of the above technical solution, preferably, in step 2, the sintering temperature is set according to the type of raw material of the thermoelectric material.

[0018] On the basis of the above technical scheme, preferably, when Bi2Te3 powder is used as the raw material of thermoelectric material, Bi2Te3 powder is used to prepare thermoelectric columns using p-type and n-type powders respectively. P-type and n-type are two types of thermoelectric materials. It should be noted that some patents currently use porous metal materials to connect p-type and n-type thermoelectric columns, but in these patents, the porous metal is set as a conductive contact. The reason is that the porous metal has a certain flexibility. The flexible conductive contact formed between the thermoelectric columns makes the device have a certain flexibility, and the flexible thermoelectric device can fit tightly to the surface of uneven objects. In the present invention, a foam metal material is used as a metal layer to separate the thermoelectric column from the conductive contact. The conductive contact can be a copper electrode on a hard ceramic substrate or other conductive materials. The above-mentioned metal layer plays the following roles:

[0019] (1) As a surface metallization layer for brazing process. Since semiconductors are often dominated by covalent bonds or ionic bonds at the microscopic level, this type of bonding material exhibits stable electronic coordination and high interface energy. This type of material is generally difficult to be wetted and welded by metal brazing filler metals with metal bonds. Therefore, a metal layer is usually grown on the upper and lower ends of the thermoelectric column to improve the welding performance. This process is called surface metallization. After sintering, the surface of the foam metal will have tiny holes. These holes enhance the capillary action of the brazing filler metal and improve the wettability of the brazing filler metal on the surface of the metal layer.

[0020] (2) Serves as a diffusion barrier to prevent the mutual diffusion of conductive contact elements and thermoelectric material elements. Thermoelectric devices usually serve in high-temperature environments, and the thermoelectric material elements and conductive contact elements will diffuse with each other, increasing the resistivity. According to Fick's diffusion law, the diffusion flux is proportional to the diffusion coefficient, and the diffusion coefficient is usually positively correlated with the temperature. Therefore, high temperature will promote the diffusion of elements inside the material. Generally speaking, high-performance thermoelectric materials are often based on heavily doped semiconductors. The diffusion of elements will reduce the doping concentration of the semiconductor and deteriorate the thermoelectric performance. For example, a paper shows that the Mg element of Mg3Bi2 thermoelectric material will diffuse to the conductive contact at high temperature, thereby forming Mg vacancies. The Mg vacancies recombine with carriers and increase the resistivity of the material. The metal layer is located between the thermoelectric column and the conductive contact. Usually, a metal that is relatively stable at high temperatures is used to prevent the mutual diffusion of thermoelectric material elements and conductive contact elements. The experiments of the present invention show that the foam metal is relatively dense inside after sintering and can act as a diffusion barrier.

[0021] (3) As a transition layer to reduce the thermal stress between the thermoelectric material and the conductive contact. The thermoelectric material is directly connected to the solder (usually tin), and the two are rigidly connected. Due to the different thermal expansion coefficients between the thermoelectric material and the solder, if they are in a free state, the deformation of the two should be different when heated to the same temperature, and the difference in deformation will increase with the increase in temperature. Because it is a rigid connection at this time, the deformation of the two should be equal. According to the theory of material mechanics, additional internal force needs to be generated at this time to maintain the same deformation. This internal force is called thermal stress. Thermoelectric devices usually work in a high temperature environment. Under cyclic conditions, thermal stress will destroy the connection between the thermoelectric column and the solder, thereby shortening the service life. Foam metal has a certain plasticity. The foam metal material is a metal layer between the thermoelectric material and the conductive contact, allowing the thermoelectric material and the conductive contact to deform within a certain range, thereby reducing thermal stress and extending the life of the device. This application will show through verification tests that the foam metal material has the potential to serve as the above-mentioned metal layer.

[0022] More preferably, when Bi2 Te3 powder is used as the raw material of thermoelectric material, in step one, the weighing mass ratio of p-type and n-type Bi2 Te3 powders is determined according to the density of the thermoelectric column blank after sintering and the formula m1 / m2=ρ1 / ρ2, wherein m1 and ρ1 represent the mass and density of p-type Bi2 Te3 respectively, and m2 and ρ2 represent the mass and density of n-type Bi2 Te3 respectively; then, the mass of the required p-type and n-type Bi2 Te3 powders is determined according to the required height of the thermoelectric column blank and the inner diameter of the graphite mold.

[0023] The thermoelectric leg and the preparation method thereof of the present invention have the following beneficial effects compared with the prior art:

[0024] (1) The present invention improves the connection strength between the metal layer and the thermoelectric material; improves the wettability of the solder on the metal layer and thus improves the connection strength of the solder joint.

[0025] (2) Compared with the physical vapor deposition method, the present invention reduces the process flow, and the use of foamed metal has a wider range of process parameter selection than the use of powder. Compared with the use of alloy powder sintering, the thickness of the metal layer is more uniform, and the thickness of the metal layer is greatly reduced, thereby improving the processing yield of micro-sized thermoelectric columns and broadening the selection range of thermoelectric device preparation processes. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0027] Figure 1 It is a three-dimensional exploded view of the thermoelectric leg of the present invention;

[0028] Figure 2 It is a schematic diagram of step 2 of the method for preparing the thermoelectric leg of the present invention;

[0029] Figure 3 The product comparison diagram of the thermoelectric leg of the present invention, wherein (a) is a cross-sectional photograph of a thermoelectric column blank prepared by sintering alloy powder and thermoelectric material together, and (b) is a cross-sectional photograph of a thermoelectric column blank prepared by using the present invention;

[0030] Figure 4 The figures are the physical pictures of the thermoelectric legs of the present invention, wherein (a) is the physical pictures of Examples 1 to 4, and (b) is the SEM image of the interface between the foam metal and the thermoelectric material in the thermoelectric column of the present invention;

[0031] Figure 5 This is a SEM image of the metal layer of the present invention.

[0032] Figure 6 The figures are comparison diagrams of the results of the micro-scale processing experiment of the present invention and optical microscope photos of the samples.

[0033] In the figure: 1. Thermoelectric column; 2. Metal layer; 3. Base plate; 4. Brazing material layer; 5. Graphite mold; 51. Press head. DETAILED DESCRIPTION

[0034] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] Example 1

[0036] like Figure 1 As shown, a thermoelectric leg of the present invention includes a thermoelectric column 1, a metal layer 2, a substrate 3 and a solder layer 4.

[0037] The thermoelectric column 1 is made of a thermoelectric material, which is a Bi-Te based alloy, specifically Bi2 Te3 powder.

[0038] Two metal layers 2 are attached to the upper and lower end surfaces of the thermoelectric column 1. The metal layers 2 are made of foam metal material. Specifically, the foam metal is foam Ni.

[0039] The two substrates 3 are arranged vertically and spaced apart, and at least one thermoelectric column 1 is arranged between the two substrates 3. The substrate 3 is a copper-clad insulating board, which is usually used as the substrate 3 of the thermoelectric device.

[0040] The solder layer 4 is arranged between the surface of the substrate 3 and the end surface of the metal layer 2 on which the thermoelectric column 1 is arranged, and is used to connect the substrate 3 and the metal layer 2 and make them in thermal contact.

[0041] like Figure 2 As shown, the thermoelectric leg of this embodiment is made by the following preparation method, including the following steps:

[0042] Step 1. According to the product requirements of the thermoelectric legs, the final required size of the thermoelectric column product is a cubic column of 4mm×4mm×4mm, so weigh 0.492g of Bi2Te3 powder. Use a graphite mold 5 with an inner diameter of 4mm to cut the foamed Ni raw material into a shape consistent with the inner diameter of the graphite mold 5. The weighed mass of the foamed Ni is 0.154g. Fill the foamed metal raw material, thermoelectric material powder and foamed metal raw material into the graphite mold 5 in sequence. The graphite mold 5 is a crucible with pressure heads 51 inserted at both ends. The above raw materials are sandwiched between the upper and lower pressure heads 51, and the sintering pressure is applied to the raw materials by the pressure head 51 during sintering.

[0043] Step 2: Place the graphite mold 5 filled with raw materials into a spark plasma sintering system for sintering. During the sintering process, apply an axial pressure of 40MPa to the raw materials in the graphite mold 5, heat up at a rate of 100℃ / min, heat to 500℃, keep warm for 10min, and then cool with the furnace to obtain the blank after sintering. Among them, the thickness of the metal layer 2 before sintering is 1mm, the porosity is 95%, and the thickness of the metal layer 2 after sintering is 0.18mm. When Bi2Te3 powder is used as the raw material for thermoelectric materials, two types of thermoelectric columns 1, p-type and n-type, are prepared respectively. When Bi2 Te3 powder is used as the raw material of thermoelectric material, since the density of the thermoelectric column 1 blank fired by p-type and n-type in step 1 is different, it is necessary to determine the weighing mass ratio of p-type and n-type Bi2 Te3 powders according to the density of the thermoelectric column 1 blank after sintering according to the formula m1 / m2=ρ1 / ρ2, where m1 and ρ1 represent the mass and density of p-type Bi2 Te3, respectively, and m2 and ρ2 represent the mass and density of n-type Bi2 Te3, respectively; then determine the mass of the required p-type and n-type Bi2 Te3 powders according to the required height of the thermoelectric column 1 blank and the inner diameter of the graphite mold 5. In this embodiment, the mass ratio of p-type to n-type is 0.88:1.

[0044] Step three, roughly grind the upper and lower surfaces of the blank, then use a wire cutting machine to cut the blank into thermoelectric legs of required sizes, and finely grind the surfaces of the thermoelectric legs.

[0045] Example 2

[0046] In this embodiment, CoSb3 is used as the thermoelectric material, with a weighing mass of 0.488 g, and foamed Ni with the same weighing mass is used as the raw material of the metal layer 2. The preparation method and conditions are the same as those in Example 1. In the final product, the thickness of the metal layer 2 before sintering is 1 mm, and the thickness after sintering is 0.19 mm.

[0047] Example 3

[0048] In this embodiment, PbTe is used as the thermoelectric material, with a weighing mass of 0.522 g, and foamed Ni with the same weighing mass is used as the raw material of the metal layer 2. The preparation method and conditions are the same as those in Example 1. In the final product, the thickness of the metal layer 2 before sintering is 1 mm, and the thickness after sintering is 0.18 mm.

[0049] Example 4

[0050] In this embodiment, SnTe is used as the thermoelectric material, with a weighing mass of 0.416 g, and foamed Ni with the same weighing mass is used as the raw material of the metal layer 2. The preparation method and conditions are the same as those in Example 1. In the final product, the thickness of the metal layer 2 before sintering is 1 mm, and the thickness after sintering is 0.18 mm.

[0051] Example 5

[0052] In this embodiment, Cu2Se is used as the thermoelectric material, with a weighing mass of 0.416 g, and foamed Ni with the same weighing mass is used as the raw material of the metal layer 2. The preparation method and conditions are the same as those in Example 1. In the final product, the thickness of the metal layer 2 before sintering is 1 mm, and the thickness after sintering is 0.17 mm.

[0053] It should be noted that half-Heusler alloy thermoelectric material is an excellent material system working in the medium and high temperature range (300-700°C), which not only has a high thermoelectric figure of merit, but also has excellent electrical transport properties. Zintl phase compounds are also called polar intermetallic compounds, which refer to compounds composed of elements containing S orbitals that are easy to lose electrons and metal or metalloid elements containing P orbitals that are easy to obtain electrons. The above two materials are excellent performance materials in the field of thermoelectric materials, but the preparation cost is high and is not suitable for large-scale production of products. Therefore, this application does not use the above two materials as raw materials for the embodiments.

[0054] Example 6

[0055] In this embodiment, Bi2 Te3 is used as the thermoelectric material, with a weighing mass of 0.492 g, and foamed Fe weighing 0.137 g is used as the raw material of the metal layer 2. The preparation method and conditions are the same as those in Example 1. In the final product, the thickness of the metal layer 2 before sintering is 1 mm, and the thickness after sintering is 0.18 mm.

[0056] Example 7

[0057] In this embodiment, Bi2 Te3 is used as the thermoelectric material, with a weighing mass of 0.492 g, and foamed Cu weighing 0.155 g is used as the raw material of the metal layer 2. The preparation method and conditions are the same as those in Example 1. In the final product, the thickness of the metal layer 2 before sintering is 1 mm, and the thickness after sintering is 0.19 mm.

[0058] Example 8

[0059] In this embodiment, Bi2 Te3 is used as the thermoelectric material, with a weighing mass of 0.492 g, and foamed Al weighing 0.046 g is used as the raw material of the metal layer 2. The preparation method and conditions are the same as those in Example 1. In the final product, the thickness of the metal layer 2 before sintering is 1 mm, and the thickness after sintering is 0.18 mm.

[0060] Example 9

[0061] In this embodiment, Bi2 Te3 is used as the thermoelectric material, with a weighing mass of 0.492 g, and foamed Ti weighing 0.078 g is used as the raw material of the metal layer 2. The preparation method and conditions are the same as those in Example 1. In the final product, the thickness of the metal layer 2 before sintering is 1 mm, and the thickness after sintering is 0.18 mm.

[0062] Example 10

[0063] In this embodiment, Bi2 Te3 is used as the thermoelectric material, with a weighing mass of 0.492g, and foamed Ti weighing 0.397g is used as the raw material of the metal layer 2. The preparation method and conditions are the same as those in Example 1. In the final product, the thickness of the metal layer 2 before sintering is 5mm, and the thickness after sintering is 1mm. The thickness of the metal layer 2 formed after sintering is too large, which reduces the connection strength between the metal layer 2 and the brazing material layer 4.

[0064] like Figure 3The comparison between the cross-sectional photographs of the thermoelectric column blank prepared by sintering alloy powder and thermoelectric material in the prior art and the cross-sectional photographs of the thermoelectric column blank prepared by sintering using the preparation method of the present application is shown, wherein (a) is prepared by the prior art, specifically (a) is a cross-sectional photograph of the thermoelectric column blank prepared by sintering Ni alloy powder and thermoelectric material, and (b) is prepared in Example 1. It can be clearly seen that the thickness of the metal layer 2 on the upper and lower end surfaces of the cross-sectional surface of the thermoelectric column in (a) is uneven; while the thickness of the upper and lower surfaces of the sintered metal layer 2 in (b) is uniform, which can adapt to large-scale production; by comparing the two, it can be found that the thickness of the metal layer 2 in (b) is greatly reduced, and the thickness uniformity is greatly improved.

[0065] like Figure 4 (a) shows the physical products obtained in Examples 1 to 4 of the present application, and (b) is a SEM image of the interface between the foam metal and the thermoelectric material in the thermoelectric column of Example 1. It can be found that a strong mechanical bite is formed between the foam metal and the thermoelectric material, thereby strengthening the surface effect of the thermoelectric material and enhancing the surface strength of the thermoelectric material. Figure 5 The SEM image of the metal layer 2 in Example 1 is shown, and it can be found that the density of the metal layer 2 after sintering is very good, which can greatly improve the shear strength of the metal layer 2.

[0066] This application uses a universal testing machine to conduct shear tests on Examples 1 to 9, and Figure 3 In (a), the thermoelectric column blank prepared by sintering Ni alloy powder and thermoelectric material together is used as a comparative example, and the data comparison in the following table is obtained.

[0067]

[0068] By comparing the shear strength data of Examples 1 to 5 with the comparative example, it can be found that the shear strength of the sample is mainly related to the strength of the thermoelectric raw material used as the preparation material. Specifically, the stronger the shear strength of the thermoelectric material, the stronger the shear strength of the sample made from it, and thus the stronger the shear strength of the metal layer 2; and by comparing the data of Examples 6 to 9, it can be seen that the strength of the preparation material used to make the metal layer 2 can also enhance the shear strength of the sample. At the same time, through the aforementioned Figure 3 It can be seen that the thickness of the metal layer 2 of the present application is thinner, which helps to strengthen the connection strength between the thermoelectric column and the substrate 3 through the solder layer 4. Therefore, the thermoelectric column of the present application is obviously superior to the thermoelectric legs prepared by the prior art.

[0069] and Figure 6The comparison chart of the results of the micro-scale processing experiment and the optical microscope photos of the samples. Among them, the comparison group used Ni powder to prepare the metal layer 2. The Ni powder metal layer 2 fell off when it was cut into micro strips with a width of less than 1 mm. The minimum processing width of the metal layer 2 prepared by the foamed Ni of the present invention reached 155μm, which is close to the minimum processing accuracy of the wire cutting machine used in the experiment, and no falling off occurred. It can be seen that the experiment proves that the foamed metal has the potential to improve the processing yield of micro-scale thermoelectric columns.

[0070] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A thermoelectric leg, characterized in that: include: Thermoelectric column (1), made of thermoelectric material; Two metal layers (2) attached to the upper and lower end surfaces of the thermoelectric column (1); The thermoelectric material is one or more of Bi-Te based alloy, CoSb3 based skutterudite, Pb-Te based alloy, Sn-Te alloy, Cu-Se alloy, Half-Heusler alloy, and Zintl phase compound, and the metal layer (2) is made of foam metal material.

2. A thermoelectric leg according to claim 1, characterized in that: The foam metal is one or more of foam Ni, foam Fe and alloys thereof, foam Cu, foam Al and foam Ti.

3. A thermoelectric leg according to claim 1, characterized in that: The thickness of the metal layer (2) before sintering is ≤5 mm, and the porosity is 90% to 95%.

4. A thermoelectric leg according to claim 3, characterized in that: The thickness of the metal layer (2) after sintering is less than 0.2 mm.

5. The thermoelectric leg according to claim 1, characterized in that: Also includes: Two substrates (3) are arranged vertically and spaced apart, and at least one thermoelectric column (1) is arranged between the two substrates (3); The solder layer (4) is arranged between the surface of the substrate (3) and the end surface of the metal layer (2) of the thermoelectric column (1), and is used to connect the substrate (3) and the metal layer (2) and bring them into thermal contact.

6. A method for preparing a thermoelectric leg, characterized in that: The following steps are involved: Step 1: According to the product requirements of the thermoelectric leg, weigh the required mass of thermoelectric material powder, cut the foam metal raw material into a shape consistent with the inner diameter of the graphite mold (5), and sequentially load the foam metal raw material, thermoelectric material powder and foam metal raw material into the graphite mold (5); Step 2: placing the graphite mold (5) filled with the raw material into a spark plasma sintering system for sintering, applying axial pressure to the raw material in the graphite mold (5) during the sintering process, and obtaining a blank after sintering; Step three, roughly grinding the upper and lower surfaces of the blank, then using a wire cutting machine to cut the blank into thermoelectric legs of required sizes, and fine grinding the surfaces of the thermoelectric legs.

7. The method for preparing a thermoelectric leg according to claim 6, characterized in that: The axial pressure applied to the raw material in step 2 is 10MPa to 40MPa.

8. The method for preparing a thermoelectric leg according to claim 6, characterized in that: In the step 2, the sintering temperature is set according to the type of raw material of the thermoelectric material.

9. The method for preparing a thermoelectric leg according to claim 6, characterized in that: When Bi2Te3 powder is used as the raw material of thermoelectric material, the Bi2Te3 powder is used to prepare thermoelectric columns (1) in p-type and n-type forms.

10. The method for preparing a thermoelectric leg according to claim 9, characterized in that: When Bi2Te3 powder is used as the raw material of thermoelectric material, in the step 1, the weight ratio of p-type and n-type Bi2Te3 powders is determined according to the density of the thermoelectric column (1) blank after sintering according to the formula m1 / m2=ρ1 / ρ2, wherein m1 and ρ1 represent the mass and density of p-type Bi2Te3 respectively, and m2 and ρ2 represent the mass and density of n-type Bi2Te3 respectively; then, the mass of the required p-type and n-type Bi2Te3 powders is determined according to the required height of the thermoelectric column (1) blank and the inner diameter of the graphite mold (5).