Textured composites and related methods of manufacture

By using composite materials made of metal substrates and fillers with hardness higher than metal substrates in motor vehicle internal combustion engines, the surface texture is formed to optimize friction performance, and the problem of increased friction under low viscosity lubricating oil is solved, and the friction coefficient is reduced and the reduction of wear improves the stability and durability of the friction film.

CN118984749APending Publication Date: 2024-11-19HORSE POWERTRAIN SOLUTIONS S L U
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380022254.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-17
Filing Date
2023-02-02
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

With low viscosity lubricating oil, friction phenomena in motor vehicles cannot be effectively reduced. Traditional friction improvement additives do not have the best effect on motor materials and coatings, resulting in increased friction between solids and premature wear.

Method used

Composite materials made of metal matrix made of iron or copper-based alloys and fillers with hardness greater than metal matrix are formed by mechanical wear or chemical erosion to form surface textures to form protrusions to improve friction performance, and to thermal spray or laser surfaces Hardening forms a coating, suitable for friction optimization in low viscosity lubricating state.

Benefits of technology

Through the surface texture treatment of the composite material, the friction coefficient is significantly reduced, friction-related wear is reduced, the stability and durability of the friction film are improved, the service life of the friction element is extended, and CO2 emissions are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118984749A_ABST
    Figure CN118984749A_ABST
Patent Text Reader

Abstract

The invention relates to a composite material comprising: a metal matrix (3) made of an iron-based or copper-based alloy; a filler (4) made of a material having a hardness greater than that of the metal matrix (3); and a surface texture comprising protrusions (5) formed by the filler (4) protruding over all or part of the surface of the composite material.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates generally to wear associated with friction between two solid bodies and, more particularly, to optimizing friction between two solid bodies to reduce wear phenomena, particularly in motor vehicle internal combustion engines under lubricated conditions.

[0002] More particularly, the present invention relates to composite materials including surface textures and methods of making such composite materials.

[0003] In order to reduce friction in motor vehicle internal combustion engines, for example the friction of the piston in the cylinder bore, increasingly fluid lubricating oils are usually used.

[0004] However, a decrease in the viscosity of the oil leads to increased friction between the solids used, causing them to wear prematurely.

[0005] Traditionally, friction improving additives, such as ZnDDP or MoDTC, are thus added to the oil in order to create a tribofilm whose function is to protect the surface and thus improve friction.

[0006] However, the materials and coatings used for frictional contacts in electric motors are not optimal for low-viscosity oils containing these additives.

[0007] The object of the present invention is therefore to remedy these drawbacks and to propose a composite material which makes it possible to optimize the friction between two solid bodies, in particular in the presence of a low-viscosity oil to which friction-modifying additives are added.

[0008] Therefore, a method for manufacturing a composite material is proposed, which composite material includes: a metal matrix made of an iron or copper-based alloy, and a filler made of a material with a hardness greater than that of the metal matrix, the method including: generating a surface texture, generating the surface texture including forming protrusions by embossing the filler on the entire or partial surface of the composite material by mechanical wear or chemical erosion.

[0009] The material of the filler has mechanical properties that resist mechanical wear or chemical attack on all or part of the surface of the composite material.

[0010] In contrast, a metal matrix having a lower hardness than the filler material does not have sufficient mechanical strength properties to resist mechanical wear or chemical attack on all or part of the surface of the composite material.

[0011] Preferably, the material hardness of the filler is greater than or equal to 550 Hv.

[0012] According to one implementation method, the metal matrix is ​​made of steel, preferably the steel contains 11.5% to 13.5% by weight of chromium, 0% to 1% by weight of manganese, 0% to 1% by weight of silicon, 0% to 0.04% by weight of phosphorus, 0% to 0.03% by weight of carbon, 0% to 0.03% by weight of sulfur and the balance of iron.

[0013] Advantageously, the filler can be made of a metallic material, preferably steel, more preferably tool steel, containing 5.5 to 6.75 weight % of tungsten, 4.5 to 5.5 weight % of molybdenum, 3.75 to 4.5 weight % of chromium, 1.75 to 2.20 weight % of vanadium, 0.8 to 1 weight % of carbon, 0.20 to 0.45 weight % of silicon, 0.15 to 0.4 weight % of manganese, 0 to 0.03 weight % of phosphorus and the balance of iron.

[0014] The invention also relates to a method of depositing a composite material as defined above on a substrate to form a coating, wherein the deposition is carried out by thermal spraying, for example by kinetic spraying using cold gas, plasma or a high-velocity oxygen flame, or by laser hard facing.

[0015] The present invention also provides a composite material comprising a metal matrix of an iron-based or copper-based alloy, a filler of a material having a hardness greater than that of the metal matrix, and a surface texture having protrusions formed by the embossed filler on all or part of the surface of the composite material.

[0016] Advantageously, the metal matrix can be made of steel, preferably the steel containing 11.5% to 13.5% by weight of chromium, 0% to 1% by weight of manganese, 0% to 1% by weight of silicon, 0% to 0.04% by weight of phosphorus, 0% to 0.03% by weight of carbon, 0% to 0.03% by weight of sulfur and the remainder iron.

[0017] Advantageously, the filler may be made of a metallic material, preferably steel, more preferably tool steel, containing 5.5 to 6.75 wt % tungsten, 4.5 to 5.5 wt % molybdenum, 3.75 to 4.5 wt % chromium, 1.75 to 2.20 wt % vanadium, 0.8 to 1 wt % carbon, 0.20 to 0.45 wt % silicon, 0.15 to 0.4 wt % manganese, 0 to 0.03 wt % phosphorus, 0 to 0.03 wt % sulfur and the balance iron.

[0018] The present invention also provides a substrate coated with the composite material as described above.

[0019] The present invention also relates to a system comprising a first part comprising a composite material as described above, all or part of the protrusions of the composite material being arranged opposite to a second part, and an oil having a viscosity less than or equal to 5W30 arranged between the composite material and the second part.

[0020] The term lubricating oil with a viscosity less than or equal to 5W30 refers to a lubricating oil having a viscosity less than or equal to 5 centistokes at -18°C and a viscosity less than or equal to 30 centistokes at 100°C.

[0021] According to one feature, all or part of the protrusions of the composite material are arranged in contact with the second portion and the oil comprises at least one friction-modifying additive, preferably chosen from ZnDDP and MoDTC.

[0022] According to one embodiment, the first part may be a friction element of a motor vehicle, such as a cylinder bore, a bearing, a crankshaft bearing, a camshaft bearing or a cam.

[0023] The invention also relates to a motor vehicle comprising a composite material as described above.

[0024] Other objects, advantages and features will appear from the following description, given purely by way of illustration and with reference to the accompanying drawings, in which:

[0025] Figure 1 is a cross-sectional view of a cylinder bore for an internal combustion engine of a motor vehicle according to an embodiment of the present invention.

[0026] Figure 2A , Figure 2B , Figure 2C and Figure 2D A system including a cylinder bore of a textured composite material in contact with a piston is shown at times T0, T1, T2, and T3, respectively.

[0027] Figure 3 The change in coefficient of friction over time measured in another pin-plane friction test is shown.

[0028] In the following, the boundary values ​​of a range of values ​​are included in the range, in particular in the expression "between".

[0029] Furthermore, the expression "at least one" used in this specification is equivalent to the expression "one or more".

[0030] Figure 1 A first part 1 is shown, comprising a coating 2 made of a composite material comprising a metal matrix 3 , a filler 4 and a surface texture comprising protrusions 5 .

[0031] In the example explained below, the first part 1 is a cylinder bore of a motor vehicle internal combustion engine, intended to cooperate with a second part 6 formed by a piston.

[0032] According to another embodiment, the first part 1 may be another friction element, such as a bearing, a crankshaft bearing, a camshaft bearing or a motor vehicle cam.

[0033] The metal base 3 is formed of an alloy selected from an iron-based alloy or a copper-based alloy.

[0034] Furthermore, the filler 4 is formed of a material having a higher hardness than the metal base material.

[0035] Furthermore, the surface texture includes protrusions 5 formed by raised fillers 4 on the surface of the composite material.

[0036] According to one aspect, the present invention relates to a method for manufacturing a composite material, the composite material comprising a metal matrix 3 made of an iron-based or copper-based alloy, and a filler 4 made of a material having a harderness than that of the metal matrix.

[0037] Furthermore, the manufacturing method comprises the processing of the texture, which consists in forming protrusions 5 by embossing a filler 4 on all or part of the surface of the composite material.

[0038] The protrusions refer to ridges or protrusions formed from the surface of the composite material by the fillers 4 of the composite material.

[0039] This texture is produced by mechanical wear or chemical erosion.

[0040] The mechanical abrasion may be performed by at least one of a grinding, polishing or warping process. Thus, a portion of the metal matrix 3 is mechanically removed, thereby exposing the filler 4 present on the surface 2a of the coating 2.

[0041] Chemically imprinting the filler 4 to form the protrusions 5 can be achieved by using a solution to dissolve the material of the metal matrix 3 at the surface 2 a of the composite material without dissolving the material of the protrusions 5 .

[0042] Furthermore, the filler 4 is formed of a material having a harder hardness than the metal base material.

[0043] The hardness of the metal matrix 3 does not impart sufficient mechanical strength properties to resist mechanical wear or chemical attack on all or part of the surface 2a of the composite material.

[0044] On the contrary, the hardness of the material of the filler 4 gives the filler 4 mechanical properties to resist mechanical wear or chemical attack on all or part of the surface 2a of the composite material.

[0045] In this way, during the step of mechanical abrasion or chemical etching, only the metal matrix is ​​removed, revealing the fillers 4 arranged on the surface of the composite material and thus forming the protuberances 5 protruding from the surface 2a of the composite material.

[0046] In order to allow the filler 4 to resist mechanical wear or chemical attack, the minimum hardness value of the material of the filler 4 is preferably equal to 550 Hv.

[0047] Preferably, the metal matrix 3 comprises steel, more preferably, the following steel: it includes 11.5 wt% to 13.5 wt% chromium, 0 wt% to 1 wt% manganese, 0 wt% to 1 wt% silicon, 0 wt% to 0.04 wt% phosphorus, 0 wt% to 0.03 wt% carbon, 0 to 0.03 wt% sulfur and the balance iron, which is called 410L stainless steel and has a ferritic structure.

[0048] The filler 4 and the protrusions 5 formed thereby are made of a material with a higher hardness than the material of the metal base 3, and this hardness difference enables it to be naturally and easily embossed during mechanical wear or chemical erosion.

[0049] Preferably, the filler 4 is made of an iron-based metal material, more preferably steel. Iron-based materials allow a good response in applications in the lubricated regime, especially with friction-modifying additives added to the lubricating oil, and promote the creation of a tribofilm.

[0050] The material of the filler 4 may comprise a tool steel conforming to the NF EN ISO 4957 standard, for example a tool steel comprising between 5.5 wt. % and 6.75 wt. % tungsten, between 4.5 wt. % and 5.5 wt. % molybdenum, between 3.75 wt. % and 4.5 wt. % chromium, between 1.75 wt. % and 2.20 wt. % vanadium, between 0.8 wt. % and 1 wt. % carbon, between 0.20 wt. % and 0.45 wt. % silicon, between 0.15 wt. % and 0.4 wt. % manganese, between 0 wt. % and 0.03 wt. % phosphorus, between 0 wt. % and 0.03 wt. % sulfur and the remainder iron, which is commonly referred to as M2 tool steel.

[0051] The mass content of each chemical element is expressed relative to the total weight of the steel in question.

[0052] According to another embodiment, the filler 4 may be made of a nickel-based or cobalt-based metal material.

[0053] According to another embodiment, the filler 4 may be made of a ceramic material, such as Al 2 O 3 , TiO 2 , ZrO 2 or Cr 2 O 3 .

[0054] Preferably, the average diameter or average equivalent diameter of the protrusions 5 is between 5 μm and 200 μm.

[0055] The shape of the protrusion 5 can be spherical, irregular, or formed into a spherical segment.

[0056] exist Figure 1 In the example shown, the filler 4 is substantially spherical particles, so that the protrusions 5 are also spherical or form spherical segments.

[0057] The spherical segment shape may be obtained as a result of a texturing step, in particular when the texturing is performed by mechanical abrasion, and / or as a result of friction between the first portion 1 and the second portion 6 causing a flattening of the fillers 4 protruding from the surface 2a of the composite coating.

[0058] Preferably, the ratio between the protrusions 5 and the metal matrix 3 at the surface 2a of the composite material is between 4% and 30%.

[0059] Preferably, the average height difference between the protrusions 5 and the textured surface 2a of the composite material is between 0.02 μm and 2 μm.

[0060] Preferably, the roughness Rz of the surface 2a of the composite material is between 0.1 μm and 1 μm.

[0061] Another aspect of the invention relates to a method for depositing a composite material as described above on a substrate to form a coating 2 .

[0062] According to one embodiment, the deposition may be achieved by thermal spraying, for example by dynamic spraying using cold gas, plasma or a high velocity oxygen flame known as HVOF (High Velocity Oxygen Fuel).

[0063] According to another embodiment, the deposition may be performed by a laser resurfacing technique, also known as "laser cladding".

[0064] In the example shown, the composite material takes the form of a coating 2 and the deposition of the composite material coating 2 on the substrate, which in this example is the first component 1 formed by a cylinder bore, is carried out by dynamic cold gas spraying.

[0065] Dynamic spraying using cold gas refers to a metallization process, more commonly known as "cold spray coating", in which the gas is accelerated to supersonic speed in a "De Laval" type nozzle. The metal composite material in powder form is introduced into the high pressure part of the nozzle and sprayed towards the substrate.

[0066] Above a certain velocity, which is characteristic of each sprayed material / substrate pair, the particles form a dense and highly adherent coating 2 upon impact.

[0067] To do this, the particles must undergo plastic deformation. The propellant gas is heated. As the temperature increases, the velocity of the gas increases, which accelerates the particles. The relative increase in the temperature of the powder particles contributes to their deformation at the point of impact.

[0068] Cold gas dynamic spray deposition results in metal composites with uniform microstructure, low porosity and high anchoring to the substrate.

[0069] The dynamic cold gas spraying technique makes it possible to obtain a composite material comprising a filler 4 uniformly distributed in a metal matrix 3 , so that the protrusions 5 are uniformly distributed on the surface 2 a of the coating 2 .

[0070] According to an alternative, the first portion 1 may be formed from a solid material made of composite material.

[0071] Solid composites can be made by casting or sintering powders.

[0072] Figure 2A , 2B , 2C and 2D show a system including a cylinder bore having a composite coating 2 disposed opposite a piston at different times T0, T1, T2 and T3.

[0073] The hole and the piston are in contact (forming a first portion 1 and a second portion 6) so that the piston forms an element that rubs against the composite material. The protrusions 5 of the textured composite material are arranged opposite the piston.

[0074] According to one example, the second portion 6 may be formed of a material including steel. The material of the second portion 6 may be treated or untreated, and may be coated or uncoated.

[0075] Furthermore, a lubricating oil having a viscosity of less than or equal to 5W30 and containing at least one friction-modifying additive is arranged between the bore and the piston for forming a protective film, also referred to as a tribofilm.

[0076] 5W30 designates an oil where 5 corresponds to the viscosity measured in centistokes at -18°C and 30 corresponds to the viscosity measured in centistokes at 100°C.

[0077] The term lubricating oil with a viscosity less than or equal to 5W30 refers to a lubricating oil having a viscosity less than or equal to 5 centistokes at -18°C and a viscosity less than or equal to 30 centistokes at 100°C.

[0078] According to one example, the lubricating oil is an oil having a viscosity less than or equal to oil 0W20, where 0 corresponds to the viscosity measured in centistokes at -18°C and 20 corresponds to the viscosity measured in centistokes at 100°C.

[0079] Preferably, the friction modifying additive is selected from ZnDDP and MoDTC.

[0080] The system Figures 2A to 2C The limit, mixed or elastohydrodynamic lubrication regime is shown in FIG. , where the cylinder bore and piston are in contact.

[0081] Figure 2A The system is shown in an initial state at time T0.

[0082] like Figure 2B As shown, at time T1, a friction film is formed on the protrusion 5. The friction film is formed by the pressure and shear of the friction improving additive in the friction contact. Once the friction film is formed, the friction coefficient is stable.

[0083] like Figure 2C As shown, at time T2, the tribofilm is also formed in the valleys, ie, on the metal substrate 3 disposed between the protrusions 5, either by forming directly therein or by forming on the protrusions 5 and then sweeping over the valleys.

[0084] Finally, at time T3, if Figure 2D As shown, the friction film is completely or partially removed from the protrusion 5. Therefore, the friction film in the depression reaches the height of the protrusion 5, and the system is stable. The friction coefficient is very low and there is no more friction-related wear between the cylinder bore and the piston.

[0085] Example 1

[0086] The first part 1 is coated with a composite material coating 2, which comprises: a composite material coating 2 having a ferrite structure and an average hardness of 335 Hv 0.01 The metal base 3 is made of 410L stainless steel and has an average hardness of 719Hv 0.01 Filler 4 made of M2 tool steel.

[0087] Coating 2 was deposited by dynamic cold gas spraying.

[0088] Then, texturing was performed on the surface 2a of the coating 2 by polishing using SiC1200 abrasive.

[0089] The textured composite material obtained had a roughness Rz of 0.5 μm and a porosity of 3%.

[0090] The average diameter of the filler 4 particles was 22 μm, and the filler 4 had a quasi-spherical shape.

[0091] The ratio between the protrusions 5 and the metal matrix 3 at the surface 2a of the composite material coating 2 was 11.1%.

[0092] The average height difference between the protrusions 5 and the metal substrate 3 at the surface 2a of the composite material coating 2 is 102 nm.

[0093] The surface 2a of the composite coating 2 was subjected to an alternating pin-plane friction test facing a 100C6 steel counter-sample in a 0W16 oil bath containing friction improving additives ZnDDP and MoDTC.

[0094] Figure 3 The variation of the coefficient of friction with time is shown.

[0095] from Figure 3 It can be seen that after only 800 seconds of testing, the system reached a stable moment T3. The friction is carried out on the protrusions 5 and the friction film protecting the metal substrate 3. The friction coefficient is very low and stable in the long term. Due to the friction film formed in this way, the wear is almost zero.

[0096] Therefore, the texture of the composite material comprising the protrusions 5 allows a significant improvement in the performance of internal combustion engines and, due to the reduction in friction, a reduction in their CO 2 emissions.

[0097] Due to the protection of the friction film, wear is reduced and the durability of the first part 1 and the second part 6 involved in the friction can be increased.

[0098] In the hydrodynamic regime (not shown) where the cylinder bore and piston are not in contact, it is the oil that applies friction according to its thickness.

[0099] In the case of friction in the hydrodynamic regime, the two solid bodies of the system do not touch because the thickness of the oil is great, for example in the middle of a cylinder stroke where the piston speed is very high. The friction is caused by shearing of the oil. The thicker the oil film, the greater the force required and therefore the greater the friction coefficient.

[0100] In the hydrodynamic state, no friction film is formed because there is no contact between the solids. Therefore, the initial texture formed by the protrusions 5 will not be changed. The presence of the protrusions 5 of the composite material can locally reduce the shear force.

[0101] Therefore, in a lubricated state where the first portion 1 and the second portion 6 are in contact, the protrusions 5 of the textured composite material may cause a friction film to form, thereby reducing friction.

[0102] In a lubricated state where the first portion 1 and the second portion 6 are not in contact, the protrusions 5 of the textured composite material can reduce shear force, thereby also reducing friction.

Claims

1. A method for manufacturing a composite material, the composite material comprising a metal matrix (3) of an iron-based or copper-based alloy, and a filler (4) of a material having a hardness greater than that of the metal matrix (3), the method comprising forming a surface texture, the forming of the surface texture comprising forming protrusions (5) by imprinting the filler (4) on the entire or partial surface of the composite material by mechanical wear or chemical erosion.

2. The method according to claim 1, wherein: The metal matrix (3) is made of steel, preferably a steel containing 11.5 to 13.5 wt. % chromium, 0 to 1 wt. % manganese, 0 to 1 wt. % silicon, 0 to 0.04 wt. % phosphorus, 0 to 0.03 wt. % carbon, 0 to 0.03 wt. % sulfur and the remainder iron.

3. The method according to claim 1 or 2, wherein: The filler (4) is made of a metal material, preferably steel, more preferably a tool steel containing 5.5 to 6.75 wt % of tungsten, 4.5 to 5.5 wt % of molybdenum, 3.75 to 4.5 wt % of chromium, 1.75 to 2.20 wt % of vanadium, 0.8 to 1 wt % of carbon, 0.20 to 0.45 wt % of silicon, 0.15 to 0.4 wt % of manganese, 0 to 0.03 wt % of phosphorus, 0 to 0.03 wt % of sulfur and the balance of iron.

4. A method for depositing a composite material according to any of the preceding claims on a substrate (1) to form a coating (2), wherein the deposition is carried out by thermal spraying, for example by dynamic cold gas, plasma or high-velocity oxygen flame spraying, or by laser surface hardening.

5. A composite material comprising a metal matrix (3) made of an iron-based or copper-based alloy, a filler (4) made of a material having a hardness greater than that of the metal matrix (3), and a surface texture comprising protrusions (5), wherein the protrusions (5) are formed by imprinting the filler (4) on the entire or partial surface of the composite material.

6. The composite material according to claim 5, wherein The metal matrix (3) is made of steel, which preferably contains: 11.5% to 13.5% by weight of chromium, 0% to 1% by weight of manganese, 0% to 1% by weight of silicon, 0% to 0.04% by weight of phosphorus, 0% to 0.03% by weight of carbon, 0% to 0.03% by weight of sulfur and the balance of iron.

7. The composite material according to claim 5 or 6, wherein: The filler (4) is made of a metal material, preferably steel, more preferably tool steel, wherein the tool steel contains 5.5 to 6.75 weight % of tungsten, 4.5 to 5.5 weight % of molybdenum, 3.75 to 4.5 weight % of chromium, 1.75 to 2.20 weight % of vanadium, 0.8 to 1 weight % of carbon, 0.20 to 0.45 weight % of silicon, 0.15 to 0.4 weight % of manganese, 0 to 0.03 weight % of phosphorus, 0 to 0.03 weight % of sulfur, and the balance is iron.

8. A substrate coated with the composite material according to any one of claims 5 to 7.

9. A system comprising: A first part (1) comprising a composite material according to any one of claims 5 to 7, wherein all or part of the protrusions (5) of the composite material are arranged opposite to a second part (6); and an oil having a viscosity less than or equal to 5W30 arranged between the composite material and the second part (6).

10. The system according to claim 9, wherein: All or part of the protrusions (5) of the composite material are in contact with the second portion, the oil comprising at least one friction modifying additive, preferably selected from ZnDDP and MoDTC.

11. The system according to claim 9 or 10, wherein: The first part (1) is a friction element of a motor vehicle, such as a cylinder bore, a bearing, a crankshaft bearing, a camshaft bearing or a cam.