Rubber composition
By adding hydrazone compounds and 3-octanylthio-1-propyltriethoxysilane to the rubber composition, combining natural rubber, carbon black and silica, the enhancement and heat resistance of existing rubber compositions are solved. The problem of insufficient performance and low combustion consumption achieves excellent performance in tire applications.
Patent Information
- Application Number
- CN202380033246.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-14
- Filing Date
- 2023-04-13
- Publication Date
- 2024-11-19
AI Technical Summary
When using natural rubber compositions, natural rubber, carbon black and silica, it is difficult to simultaneously improve the reinforcement, heat resistance and low combustion properties.
Add hydrazone compounds and 3-octanylthio-1-propyltriethoxysilane to the natural rubber to form a composition containing rubber components, hydrazone compounds, carbon black and silica, and the rubber is enhanced by combining these components enhancement, heat resistance and low fuel consumption.
It realizes the enhancement, heat resistance and low combustion consumption of the rubber composition in tire applications, and is suitable for tires of high load vehicles, reducing rolling resistance and heating properties.
Smart Images

Figure BDA0005076723200000061 
Figure BDA0005076723200000091 
Figure BDA0005076723200000161
Abstract
Description
Technical Field
[0001] The present invention relates to rubber compositions. Background Art
[0002] In rubber compositions used for tires, natural rubber (NR) with excellent strength and durability is used as the mainstream rubber, and development of rubber compositions with better fuel efficiency is currently underway. In recent years, in rubber compositions used for tires, there is a tendency to add carbon black as a filler to NR and further mix a certain amount of silica for the purpose of further imparting fuel efficiency. In such a mixing system of carbon black and silica in NR, it is also expected to develop a rubber composition with further improved fuel efficiency.
[0003] Patent Document 1 discloses a method for producing a rubber composition, which comprises a rubber component (A) containing at least one selected from natural rubber and synthetic diene rubber, a filler containing an inorganic filler (B), a silane coupling agent (C), and a hydrazide compound (D), wherein the rubber composition is kneaded in multiple stages, and in the first stage of kneading, the rubber component (A), all or a part of the inorganic filler (B), all or a part of the silane coupling agent (C), and the hydrazide compound (D) are kneaded.
[0004] Patent Document 2 discloses a method for producing a rubber composition, which comprises: a first kneading stage of kneading a rubber component (A) containing a natural rubber and a modified conjugated diene polymer having at least one nitrogen-containing functional group and at least one filler (B); a second kneading stage of kneading a hydrazide compound (C) into the rubber composition obtained in the first kneading stage; and a final kneading stage of kneading a vulcanizing agent and a vulcanization accelerator into the rubber composition obtained in the second kneading stage.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Laid-Open No. 2013-144761
[0008] Patent Document 2: Japanese Patent Application Laid-Open No. 2014-005381 Summary of the invention
[0009] Problems to be solved by the invention
[0010] The present invention has been made in view of the above circumstances, and aims to solve the above-mentioned various problems in the past and achieve the following objects.
[0011] An object of the present invention is to provide a rubber composition, in which, when carbon black and silica are added to NR, the reinforcement and heat resistance are improved, and the fuel efficiency is also improved.
[0012] Means for solving problems
[0013] The inventors of the present application have conducted intensive studies to achieve the above-mentioned purpose, and as a result, have found that by combining a hydrazone compound and 3-octanoylthio-1-propyltriethoxysilane (silane coupling agent) in a rubber composition in which carbon black and silica are blended with NR, a rubber composition having improved reinforcement and heat resistance and also improved fuel efficiency can be obtained, for example, in tire applications.
[0014] The inventors of the present application have further conducted studies based on the above findings and have completed the present invention.
[0015] That is, the rubber composition of the present invention includes the following rubber composition containing a rubber component, a hydrazone compound, carbon black, silica, and 3-octanoylthio-1-propyltriethoxysilane.
[0016] Item 1.
[0017] A rubber composition comprising a rubber component, a hydrazone compound, carbon black, silica, and 3-octanoylthio-1-propyltriethoxysilane.
[0018] The rubber component contains 50 parts by mass or more of natural rubber per 100 parts by mass of the rubber component.
[0019] With respect to 100 parts by mass of the rubber component,
[0020] Containing 0.1 to 2 parts by mass of the above-mentioned hydrazone compound,
[0021] Containing 15 to 60 parts by mass of the aforementioned carbon black,
[0022] The silicon dioxide is contained in an amount of 18 to 80 parts by mass.
[0023] The 3-octanoylthio-1-propyltriethoxysilane is contained in an amount of 3 to 10 parts by mass based on 100 parts by mass of the silica.
[0024] Item 2.
[0025] The rubber composition according to item 1 above, wherein the hydrazone compound is selected from 3-hydroxy-N'-(1,3-dimethylbutylene)-2-naphthoic acid hydrazide, 3-hydroxy-2-naphthoic acid hydrazide, N'-(1-methylethylidene) salicylic acid hydrazide, N'-(1-methylpropylidene) salicylic acid hydrazide, N'-(1,3-dimethylbutylidene) salicylic acid hydrazide, N'-(2-furylmethylene) salicylic acid hydrazide, 1-hydroxy-N'-(1-methylethylidene)-2-naphthoic acid hydrazide, 1-hydroxy At least one hydrazone compound selected from the group consisting of 1-hydroxy-N'-(1-methylpropylene)-2-naphthoic acid hydrazide, 1-hydroxy-N'-(1,3-dimethylbutylene)-2-naphthoic acid hydrazide, 1-hydroxy-N'-(2-furylmethylene)-2-naphthoic acid hydrazide, 3-hydroxy-N'-(1-methylethylidene)-2-naphthoic acid hydrazide, 3-hydroxy-N'-(1-methylpropylene)-2-naphthoic acid hydrazide, and 3-hydroxy-N'-(2-furylmethylene)-2-naphthoic acid hydrazide.
[0026] Item 3.
[0027] The rubber composition as described in the above item 1, wherein the hydrazone compound is 3-hydroxy-N′-(1,3-dimethylbutylidene)-2-naphthoic acid hydrazide.
[0028] Effects of the Invention
[0029] When the rubber composition of the present invention is used in tires, for example, carbon black and silica are added to NR to improve reinforcement and heat resistance, and also improve fuel efficiency. DETAILED DESCRIPTION
[0030] The present invention is described in detail below.
[0031] The embodiments of the present invention are provided to facilitate better understanding of the gist of the invention and do not limit the content of the invention unless otherwise specified.
[0032] In the present specification, “including” and “containing” are concepts covering all cases of “including (comprise)”, “consist essentially of”, and “consist of (consist of)”.
[0033] In the present specification, when a numerical range is expressed as "A to B", it means not less than A and not more than B.
[0034] [1] Rubber composition
[0035] The rubber composition of the present invention comprises a rubber component, a hydrazone compound, carbon black, silica, and 3-octanoylthio-1-propyltriethoxysilane.
[0036] The rubber composition contains 50 parts by mass or more of natural rubber per 100 parts by mass of the rubber component.
[0037] The rubber composition contains 0.1 to 2 parts by mass of a hydrazone compound, 15 to 60 parts by mass of carbon black, and 18 to 80 parts by mass of silica, based on 100 parts by mass of the rubber component.
[0038] The rubber composition contains 3 to 10 parts by mass of 3-octanoylthio-1-propyltriethoxysilane based on 100 parts by mass of silica.
[0039] In the rubber composition of the present invention, the hydrazone compound is preferably 3-hydroxy-N′-(1,3-dimethylbutylidene)-2-naphthoic acid hydrazide.
[0040] When the rubber composition of the present invention is used in tires, for example, carbon black and silica are added to NR to improve reinforcement and heat resistance, and also improve fuel efficiency.
[0041] The rubber composition of the present invention is useful as a rubber composition for heavy-duty tires for high-load trucks, buses, aircraft, industrial vehicles, and the like, in tire applications, particularly truck tire applications and bus tire applications.
[0042] [1-1] Rubber components
[0043] The rubber composition of the present invention contains a rubber component, and the rubber component contains 50 parts by mass or more of natural rubber per 100 parts by mass of the rubber component.
[0044] As the natural rubber (NR), natural rubber latex, technical standard rubber (TSR), smoked rubber sheet (RSS), gutta-percha, natural rubber derived from eucommia, natural rubber derived from guayule, natural rubber derived from rubber grass, and the like are preferable.
[0045] NR includes modified natural rubbers such as epoxidized natural rubber, methacrylic acid-modified natural rubber, and styrene-modified natural rubber obtained by modifying these natural rubbers.
[0046] As rubber components other than NR, various synthetic diene rubbers can be used. As synthetic diene rubbers, preferably butadiene rubber (BR), styrene-butadiene copolymer rubber (SBR), isoprene rubber (IR), nitrile rubber (NBR), chloroprene rubber (CR), ethylene-propylene-diene terpolymer rubber (EPDM), styrene-isoprene-styrene terblock copolymer (SIS), styrene-butadiene-styrene terblock copolymer (SBS), etc., and modified synthetic diene rubbers thereof can be cited.
[0047] The modified synthetic diene rubber includes diene rubber obtained by modification methods such as main chain modification, single terminal modification, double terminal modification, etc. Here, various functional groups such as epoxy, amino, alkoxysilyl, and hydroxyl groups can be cited as the modifying functional groups of the modified synthetic diene rubber, and the modified synthetic diene rubber may contain one or more of these functional groups.
[0048] The method for producing the synthetic diene rubber is not particularly limited, and examples thereof include emulsion polymerization, solution polymerization, radical polymerization, anionic polymerization, cationic polymerization, etc. The glass transition temperature of the synthetic diene rubber is also not particularly limited.
[0049] As the rubber component other than NR, from the viewpoint of achieving both abrasion resistance and processability, it is preferable to use a rubber component such as BR, IR, or SBR, and it is more preferable to use BR.
[0050] There is no particular restriction on the ratio of cis / trans / vinyl in the double bond part of synthetic diene rubbers such as NR and BR, and any ratio can be used appropriately. In addition, there is no particular restriction on the number average molecular weight and molecular weight distribution of synthetic diene rubbers such as BR, but it is preferred that the number average molecular weight is 500 to 3,000,000 and the molecular weight distribution is 1.5 to 15.
[0051] As the rubber component other than the synthetic diene rubber such as NR and BR, polysulfide rubber, silicone rubber, fluororubber, and urethane rubber can be used.
[0052] As the rubber component, in addition to NR, at least one rubber component selected from the group consisting of the above-mentioned rubber components may be used, or two or more rubber components may be mixed (blended) for use.
[0053] As the rubber component other than NR, it is preferable to use a blend of NR and BR, or to use IR, SBR or the like in combination with NR and BR.
[0054] The content of NR in 100 parts by mass of the rubber component is 50 parts by mass or more, preferably 60 parts by mass or more. The rubber component may be composed of NR alone.
[0055] When BR is used in combination with NR in 100 parts by mass of the rubber component, the total content of NR and BR is preferably 80 parts by mass or more, more preferably 90 parts by mass or more. The rubber component may be composed only of NR and BR.
[0056] In the rubber composition of the present invention, by adopting the above-mentioned configuration as the composition of the rubber component, it is possible to achieve both wear resistance and low heat generation properties.
[0057] [1-2] Hydrazone compounds
[0058] The rubber composition of the present invention contains a hydrazone compound, and contains 0.1 to 2 parts by mass of the hydrazone compound based on 100 parts by mass of the rubber component.
[0059] Preferred hydrazone compounds include 3-hydroxy-N'-(1,3-dimethylbutylene)-2-naphthoic acid hydrazide, 3-hydroxy-2-naphthoic acid hydrazide, N'-(1-methylethylidene) salicylhydrazide, N'-(1-methylpropylidene) salicylhydrazide, N'-(1,3-dimethylbutylidene) salicylhydrazide, N'-(2-furylmethylene) salicylhydrazide, 1-hydroxy-N'-(1-methylethylidene)-2-naphthoic acid hydrazide, 1-hydroxy -N'-(1-methylpropylene)-2-naphthoic acid hydrazide, 1-hydroxy-N'-(1,3-dimethylbutylene)-2-naphthoic acid hydrazide, 1-hydroxy-N'-(2-furylmethylene)-2-naphthoic acid hydrazide, 3-hydroxy-N'-(1-methylethylidene)-2-naphthoic acid hydrazide, 3-hydroxy-N'-(1-methylpropylene)-2-naphthoic acid hydrazide, 3-hydroxy-N'-(2-furylmethylene)-2-naphthoic acid hydrazide, etc.
[0060] As the hydrazone compound, at least one hydrazone compound selected from the group consisting of the above-mentioned hydrazone compounds may be used. One of these hydrazone compounds may be used alone, or two or more of them may be mixed (blended) and used.
[0061] The hydrazone compound is more preferably 3-hydroxy-N′-(1,3-dimethylbutylidene)-2-naphthoylhydrazide.
[0062] [Chemical formula 1]
[0063]
[0064] In the rubber composition of the present invention, when 3-octanoylthio-1-propyltriethoxysilane is blended into the rubber composition containing NR, carbon black and silica, a hydrazone compound is further blended to improve the reactivity of 3-octanoylthio-1-propyltriethoxysilane with silica or NR.
[0065] As a result, the reinforcing properties and fuel efficiency of the rubber composition of the present invention can be improved, and the heat resistance can also be improved by adding the hydrazone compound.
[0066] In the rubber composition of the present invention,
[0067] The rubber composition contains 0.1 to 2 parts by mass of the hydrazone compound per 100 parts by mass of the rubber component. The rubber composition contains preferably 0.5 to 1.5 parts by mass of the hydrazone compound per 100 parts by mass of the rubber component.
[0068] When the content of the hydrazone compound is 0.1 to 2 parts by mass, the processability of the rubber composition is good, and when the rubber composition is used as a tire, excellent fuel efficiency (rolling resistance performance) is exhibited.
[0069] [1-3] Carbon black
[0070] The rubber composition of the present invention contains carbon black, and contains 15 to 60 parts by mass of carbon black relative to 100 parts by mass of the rubber component. By including carbon black in the rubber component, the electrical resistance of the rubber can be reduced, thereby obtaining an effect of suppressing static electricity and further improving the strength of the rubber.
[0071] Examples of carbon black include high, medium or low structure SAF, ISAF, IISAF, N110, N134, N220, N234, N330, N339, N375, N550, HAF, FEF, GPF and SRF grade carbon blacks. Among them, preferred carbon blacks include SAF, ISAF, IISAF, N134, N234, N330, N339, N375, HAF and FEF grade carbon blacks.
[0072] The DBP absorption of carbon black is not particularly limited, but is preferably 60 cm 3 / 100g~200cm 3 / 100g, preferably 70cm 3 / 100g~180cm 3 / 100g or more, more preferably 80cm 3 / 100g~160cm 3 / 100g.
[0073] Nitrogen adsorption specific surface area of carbon black (N 2 SA, measured according to JIS K6217-2: 2001) is preferably 30 m 2 / g~200m 2 / g, more preferably 40m 2 / g~180m 2 / g, more preferably 50m 2 / g~160m 2 / g.
[0074] As the carbon black, commercially available carbon black can be used, and for example, a carbon-silica dual phase filler can be used.
[0075] As the carbon black, at least one compound selected from the group consisting of the above-mentioned carbon blacks may be used. One of these carbon blacks may be used alone, or two or more thereof may be mixed (blended) and used.
[0076] In the rubber composition, the amount of carbon black is 15 to 60 parts by mass, preferably 20 to 50 parts by mass, and more preferably 25 to 40 parts by mass, relative to 100 parts by mass of the rubber component. In the rubber composition, by making the amount of carbon black 15 to 60 parts by mass relative to 100 parts by mass of the rubber component, the processability of the rubber composition is good, and when the rubber composition is used as a tire, the coloring is good.
[0077] [1-4] Silica
[0078] The rubber composition of the present invention contains silica, and contains 18 to 80 parts by mass of silica based on 100 parts by mass of the rubber component.
[0079] As the silica, wet silica, dry silica or colloidal silica is preferably used, and wet silica is more preferably used. The surface of these silicas may be subjected to an organic treatment in order to improve the affinity with the rubber component.
[0080] The BET specific surface area of silica is not particularly limited, and for example, 40 m 2 / g~350m 2 The silica having a BET specific surface area within this range has the advantage of being able to simultaneously achieve rubber reinforcement and dispersibility in rubber components. The BET specific surface area is measured in accordance with ISO5794 / 1.
[0081] From this viewpoint, the preferred silica has a BET specific surface area of 80 m 2 / g~300m 2 The silica is preferably in the range of 100 m / g, and more preferably has a BET specific surface area of 100 m 2 / g~270m 2 / g of silica, particularly preferably with a BET specific surface area of 110m 2 / g~270m2 / g of silica.
[0082] Commercially available silica includes "HD165MP" (BET specific surface area = 165 m 2 / g), "HD115MP" (BET specific surface area = 115m 2 / g), "HD200MP" (BET specific surface area = 200m 2 / g), "HD250MP" (BET specific surface area = 250m 2 / g), trade name "Nipsil AQ" manufactured by Tosoh Silica Corporation (BET specific surface area = 205 m 2 / g), “Nipsil KQ” (BET specific surface area = 240 m 2 / g), Degussa AG's trade name "Ultrasil VN3" (BET specific surface area = 175 m 2 / g) etc.
[0083] As the silica, at least one compound selected from the group consisting of the above-mentioned silicas can be used. One of these silicas can be used alone, or two or more of them can be mixed (blended) for use.
[0084] In the rubber composition, the amount of silica blended is 18 to 80 parts by mass, preferably 19 to 45 parts by mass, and more preferably 20 to 40 parts by mass, relative to 100 parts by mass of the rubber component. In the rubber composition, by making the amount of silica blended to 18 to 80 parts by mass relative to 100 parts by mass of the rubber component, low heat generation and wear resistance of the rubber composition can be achieved at the same time.
[0085] [1-5] Silane coupling agent
[0086] The rubber composition of the present invention contains 3-octanoylthio-1-propyltriethoxysilane as a silane coupling agent in addition to silica, and contains 3 to 10 parts by mass of 3-octanoylthio-1-propyltriethoxysilane based on 100 parts by mass of silica.
[0087] [Chemical formula 2]
[0088]
[0089] By adding a silane coupling agent, the reinforcement of the rubber composition can be improved, or the tear strength and abrasion resistance of the rubber composition can be improved.
[0090] In the rubber composition of the present invention, when carbon black and silica are added to NR, 3-octanoylthio-1-propyltriethoxysilane is added together with a hydrazone compound, thereby improving reinforcement and fuel efficiency and also improving heat resistance.
[0091] The rubber composition of the present invention may be blended in combination with other silane coupling agents, titanate coupling agents, aluminate coupling agents, and zirconate coupling agents.
[0092] There are no particular restrictions on the silane coupling agent, and commercially available products can be preferably used. Examples of the silane coupling agent include sulfide-based, polysulfide-based, thioester-based, thiol-based, olefin-based, epoxy-based, amino-based, and alkyl-based silane coupling agents. As the silane coupling agent, bis(3-triethoxysilylpropyl)tetrasulfide is preferably used.
[0093] The titanate coupling agent is not particularly limited, and a commercially available product can be preferably used. Examples of the titanate coupling agent include alkoxide-based, chelate-based, and acylate-based titanate coupling agents.
[0094] The aluminate coupling agent is not particularly limited, and a commercially available one can be preferably used.
[0095] The zirconate coupling agent is not particularly limited, and a commercially available product can be preferably used. Examples of the zirconate coupling agent include alkoxide-based, chelate-based, and acylate-based zirconate coupling agents.
[0096] As other silane coupling agents, titanate coupling agents, aluminate coupling agents, and zirconate coupling agents, at least one compound selected from the group consisting of the above compounds can be used. One of these compounds can be used alone, or two or more thereof can be mixed (blended) and used.
[0097] In the rubber composition, the amount of 3-octanoylthio-1-propyltriethoxysilane blended is 3 to 10 parts by mass, preferably 4 to 9 parts by mass, and more preferably 5 to 8 parts by mass, relative to 100 parts by mass of silica.
[0098] In the rubber composition, by setting the blending amount of 3-octanoylthio-1-propyltriethoxysilane to 3 to 10 parts by mass relative to 100 parts by mass of silica, 3-octanoylthio-1-propyltriethoxysilane is blended together with a hydrazone compound when carbon black and silica are blended into NR, thereby improving reinforcement and fuel efficiency, and also improving heat resistance.
[0099] [1-6] Other compounding agents
[0100] The rubber composition of the present invention may appropriately contain, in addition to the aforementioned components, inorganic fillers other than carbon black and silica, vulcanizers, vulcanization accelerators, vulcanization accelerator aids, antioxidants, softeners, plasticizers, scorch retarders, antiozonants, foaming agents, vulcanization retarders, and other compounding agents commonly used in the rubber industry.
[0101] Inorganic fillers
[0102] As an inorganic filler, calcium carbonate (CaCO 3 ), aluminum oxide (Al 2 O 3 ), alumina hydrate (Al 2 O 3 ·H 2 O), aluminum hydroxide [Al(OH) 3 ]、Aluminum carbonate [Al 2 (CO 3 ) 3 ]、Magnesium hydroxide [Mg(OH) 2 ], magnesium oxide (MgO), magnesium carbonate (MgCO 3 )、Talc(3MgO·4SiO 2 ·H 2 O), attapulgite (5MgO·8SiO 2 9H 2 O), titanium dioxide (TiO 2 )、TiO 2n-1 ), calcium oxide (CaO), calcium hydroxide [Ca(OH) 2 ]、MgO·Al 2 O 3 ), clay (Al 2 O 3 ·2SiO 2 ), kaolin (Al 2 O 3 ·2SiO 2 ·2H 2 O), pyrophyllite (Al 2 O 3 ·4SiO 2 ·H 2 O), bentonite (Al 2 O 3 ·4SiO 2 ·2H 2 O), aluminum silicate (Al 2 SiO 5 、Al 4 ·3SiO 4 ·5H 2 O, etc.), magnesium silicate (Mg2 SiO 4 MgSiO 3 etc.), calcium silicate (Ca 2 ·SiO 4 Calcium aluminum silicate (Al 2 O 3 ·CaO·2SiO 2 etc.), calcium magnesium silicate (CaMgSiO 4 )、ZrO 2 ), zirconium hydroxide [ZrO(OH) 2 ·nH 2 O], zirconium carbonate [Zr(CO 3 ) 2 ], zinc acrylate, zinc methacrylate, various zeolites containing charge-compensating hydrogen, crystalline aluminosilicates of alkali metals or alkaline earth metals, and the like.
[0103] As the inorganic filler, at least one inorganic filler selected from the group consisting of the above-mentioned inorganic fillers can be used. These inorganic fillers can be used alone or in combination of two or more.
[0104] Vulcanizing agent
[0105] As the vulcanizing agent, an organic peroxide or a sulfur-based vulcanizing agent may be added.
[0106] As the organic peroxide, for example, benzoyl peroxide, diisopropylbenzene peroxide, di-tert-butyl peroxide, tert-butyl isopropylbenzene peroxide, methyl ethyl ketone peroxide, isopropylbenzene hydroperoxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, 2,5-dimethyl-2,5-di(benzoyl peroxy)hexane, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3, 1,3-bis(tert-butylperoxypropyl)benzene, di-tert-butylperoxy-diisopropylbenzene, tert-butylbenzene peroxide, 2,4-dichlorobenzoyl peroxide, 1,1-di-tert-butylperoxy-3,3,5-trimethylsiloxane, 4,4-di-tert-butylperoxyvalerate, etc. are preferably used. Among the organic peroxides, diisopropylbenzene peroxide, tert-butylbenzene peroxide, and di-tert-butylperoxy-diisopropylbenzene are preferred.
[0107] As the sulfur-based vulcanizing agent, for example, sulfur, morpholine disulfide, etc. can be blended. Among the sulfur-based vulcanizing agents, sulfur is preferred.
[0108] As the vulcanizing agent, at least one vulcanizing agent selected from the group consisting of the above-mentioned vulcanizing agents can be used. One of these vulcanizing agents can be used alone, or two or more of them can be mixed (blended) and used.
[0109] Vulcanization accelerator
[0110] As the vulcanization accelerator, a sulfenamide-based, thiazole-based, thiuram-based, thiourea-based, guanidine-based, dithiocarbamic acid-based, aldehyde-amine-based or aldehyde-ammonia-based accelerator may be added.
[0111] As a vulcanization accelerator, stearic acid, zinc white (zinc oxide) and the like may be added.
[0112] The vulcanization accelerator and the vulcanization accelerator aid may be at least one vulcanization accelerator and vulcanization accelerator aid selected from the group consisting of the above-mentioned vulcanization accelerators and vulcanization accelerator aids. One of these vulcanization accelerators and vulcanization accelerator aids may be used alone, or two or more thereof may be mixed (blended) and used.
[0113] Anti-aging agents
[0114] As the anti-aging agent, amine-based, phenol-based, imidazole-based compounds, metal carbamates, waxes, etc. may be added.
[0115] As the anti-aging agent, at least one anti-aging agent selected from the group consisting of the above-mentioned anti-aging agents can be used. These anti-aging agents can be used alone or in combination of two or more.
[0116] Softener
[0117] As softeners, petroleum-based softeners such as process oil, lubricating oil, paraffin, liquid paraffin, petroleum asphalt, and vaseline; fatty oil-based softeners such as castor oil, linseed oil, rapeseed oil, and coconut oil; waxes such as tall oil, factice, beeswax, carnauba wax, and lanolin; fatty acids such as linoleic acid, palmitic acid, stearic acid, and lauric acid, etc. can be used.
[0118] As the softener, at least one softener selected from the group consisting of the above-mentioned softeners can be used. These softeners can be used alone or in the form of a mixture (blended) of two or more.
[0119] By adding a softener, the kneading processability can be further improved.
[0120] Plasticizers
[0121] As the plasticizer, DMP (dimethyl phthalate), DEP (diethyl phthalate), DBP (dibutyl phthalate), DHP (diheptyl phthalate), DOP (dioctyl phthalate), DINP (diisononyl phthalate), DIDP (diisodecyl phthalate), BBP (butyl benzyl phthalate), DLP (dilauryl phthalate), DCHP (dicyclohexyl phthalate), hydrogenated phthalic anhydride ester, DOZ (di-2-ethylhexyl azelate), DBS (dibutyl sebacate), DOS (dioctyl sebacate), acetylcitrate triethyl, acetylcitrate tributyl, DBM (dibutyl maleate), DOM (2-ethylhexyl maleate), DBF (dibutyl fumarate) and the like can be added.
[0122] As the plasticizer, at least one plasticizer selected from the group consisting of the above-mentioned plasticizers can be used. These plasticizers can be used alone or in combination of two or more.
[0123] Anti-scorch agent
[0124] As the scorch retarder, organic acids such as phthalic anhydride, salicylic acid, and benzoic acid; nitroso compounds such as N-nitrosodiphenylamine; and N-cyclohexylthiophthalimide may be added.
[0125] As the scorch retarder, at least one scorch retarder selected from the group consisting of the above-mentioned scorch retarders can be used. One of these scorch retarders can be used alone, or two or more of them can be mixed (blended) for use.
[0126] [2] Method for producing rubber composition
[0127] In the method for producing the rubber composition of the present invention, when carbon black and silica are added to NR, 3-octanoylthio-1-propyltriethoxysilane and a hydrazone compound are added together to improve the reactivity of 3-octanoylthio-1-propyltriethoxysilane with silica.
[0128] As a result, the rubber composition of the present invention has improved reinforcement and fuel economy, and also has improved heat resistance due to the addition of the hydrazone compound.
[0129] The rubber composition of the present invention is obtained by kneading the compounding ingredients using a kneading machine such as an open kneading machine such as a roll or a closed kneading machine such as a Banbury mixer. After the rubber composition is molded, it is vulcanized at 140° C. to 190° C. for 5 minutes to 120 minutes, and thus can also be applied to various rubber products.
[0130] [3] Tires
[0131] The rubber composition of the present invention is preferably used in a tire, and can be used in particular for various parts such as a tire tread, an undertread, a carcass, a sidewall, and a bead portion.
[0132] The tire of the present invention has low heat build-up, thereby reducing the rolling resistance of the tire and having excellent low fuel consumption. In addition, the tire has excellent tolerance to high loads and can be suitably used as a tire for heavy-duty vehicles such as trucks, buses, aircraft or industrial vehicles (heavy-duty tires).
[0133] Although the embodiments of the present invention have been described above, the present invention is not limited to these examples and can be implemented in various forms without departing from the gist of the present invention.
[0134] Example
[0135] Hereinafter, embodiments of the present invention will be described in more detail based on examples.
[0136] The present invention is not limited thereto.
[0137] [1] Production of rubber composition (test composition)
[0138] The components described in Table 1 below were mixed at their respective ratios (parts by mass), and kneaded for 5 minutes using a plastomill while adjusting the rotation speed so that the maximum temperature of the mixture became 160° C., thereby producing each rubber composition.
[0139] [2] Evaluation test of rubber composition
[0140] The rubber compositions prepared in the respective Examples and Comparative Examples were evaluated for low heat build-up properties, reinforcement properties, and heat resistance.
[0141] (1) Low heat generation (tanδ index)
[0142] The rubber composition prepared in each of the Examples and Comparative Examples was vulcanized at 150° C. for 25 minutes to obtain a vulcanized rubber.
[0143] The loss tangent (tan δ) of the obtained vulcanized rubber was measured using a viscoelasticity measuring apparatus (manufactured by TA Instruments) under the conditions of room temperature, a dynamic strain of 5%, and a frequency of 15 Hz.
[0144] In the evaluation, the low heat build-up property based on the loss tangent (tan δ) of the rubber composition of each sample was expressed as a low heat build-up property index and was expressed as an index whose reciprocal value when the tan δ value of Comparative Example 1 was set to 100.
[0145] A larger value of the low heat buildup index indicates better low heat buildup properties.
[0146] (2) Enhancement
[0147] The 300% modulus of the rubber composition prepared in each of the Examples and Comparative Examples was measured in accordance with JIS K6251 in a dumbbell type No. 3 test at room temperature and under the condition of 500 mm / min.
[0148] In the evaluation, the reinforcing property based on the 300% modulus of the rubber composition of each sample was expressed as a reinforcing property index, and was expressed as an index when the value of the 300% modulus of Comparative Example 1 was set to 100.
[0149] A larger value of the reinforcing index indicates better reinforcing properties.
[0150] (3) Heat resistance
[0151] The rubber composition prepared in each of the Examples and Comparative Examples was deteriorated in a Geer oven at 100° C. for 72 hours, and the change in tensile strength was measured by a tensile test in accordance with JIS K6257.
[0152] In the evaluation, the heat resistance based on the change in tensile strength of the rubber composition of each sample was expressed as a heat resistance index, and was expressed as an index when the value of the change in tensile strength in the tensile test of Comparative Example 1 was set to 100.
[0153] A larger value of the heat resistance index indicates better heat resistance.
[0154] The results are shown in Tables 1 to 4.
[0155] [Table 1]
[0156]
[0157] [Table 2]
[0158]
[0159] [Table 3]
[0160]
[0161] [Table 4]
[0162]
[0163] Natural rubber: TSR-20 made by GUANGKEN RUBBER
[0164] Butadiene rubber: manufactured by Ube Industries, Ltd., trade name "BR150B"
[0165] Carbon black: N234 grade
[0166] Silicon dioxide: manufactured by Tosoh Silica Corporation, trade name "Nipsil (brand AQ)"
[0167] Hydrazone compound: 3-hydroxy-N'-(1,3-dimethylbutylidene)-2-naphthoylhydrazide
[0168] Silane coupling agent 1: 3-octanoylthio-1-propyltriethoxysilane
[0169] Silane coupling agent 2: bis(3-triethoxysilylpropyl) disulfide
[0170] Anti-aging agent: N-phenyl-N'-(1,3-dimethylbutyl) p-phenylenediamine (6-PPD)
[0171] Wax: Rhein Chemie Rheinau, trade name "Antilux111"
[0172] Vulcanization accelerator: N-cyclohexyl-2-benzothiazole sulfenamide (CBS)
[0173] In the rubber composition of the examples, when carbon black and silica are blended into NR, 3-octanoylthio-1-propyltriethoxysilane and a hydrazone compound are blended together, thereby improving reinforcement and fuel efficiency, and heat resistance is also improved by blending the hydrazone compound.
[0174] Industrial Applicability
[0175] The rubber composition of the present invention contains a hydrazone compound and 3-octanoylthio-1-propyltriethoxysilane (silane coupling agent) in combination in a rubber composition in which carbon black and silica are blended in NR, thereby obtaining a rubber composition having improved reinforcement and heat resistance in tire applications, for example, and also improved fuel efficiency.
[0176] The rubber composition of the present invention is useful as a rubber composition for heavy-duty tires for high-load trucks, buses, aircraft, industrial vehicles, and the like, in tire applications, particularly truck tire applications and bus tire applications.
Claims
1. A rubber composition comprising a rubber component, a hydrazone compound, carbon black, silica, and 3-octanoylthio-1-propyltriethoxysilane, The rubber component contains 50 parts by mass or more of natural rubber per 100 parts by mass of the rubber component. With respect to 100 parts by mass of the rubber component, Containing 0.1 to 2 parts by mass of the hydrazone compound, Containing 15 to 60 parts by mass of the carbon black, comprising 18 to 80 parts by mass of the silicon dioxide, With respect to 100 parts by mass of the silicon dioxide, The 3-octanoylthio-1-propyltriethoxysilane is contained in an amount of 3 parts by mass to 10 parts by mass.
2. The rubber composition according to claim 1, in, The hydrazone compound is selected from 3-hydroxy-N'-(1,3-dimethylbutylene)-2-naphthoic acid hydrazide, 3-hydroxy-2-naphthoic acid hydrazide, N'-(1-methylethylidene) salicylic acid hydrazide, N'-(1-methylpropylidene) salicylic acid hydrazide, N'-(1,3-dimethylbutylidene) salicylic acid hydrazide, N'-(2-furylmethylene) salicylic acid hydrazide, 1-hydroxy-N'-(1-methylethylidene)-2-naphthoic acid hydrazide, 1-hydroxy-N'-(1-hydroxypropylidene)-2-naphthoic acid hydrazide, At least one hydrazone compound selected from the group consisting of 1-hydroxy-N'-(1,3-dimethylbutylene)-2-naphthoic acid hydrazide, 1-hydroxy-N'-(2-furylmethylene)-2-naphthoic acid hydrazide, 3-hydroxy-N'-(1-methylethylidene)-2-naphthoic acid hydrazide, 3-hydroxy-N'-(1-methylpropylene)-2-naphthoic acid hydrazide, and 3-hydroxy-N'-(2-furylmethylene)-2-naphthoic acid hydrazide.